A kind of corrosion-resistant plywood and preparation method thereof

By using lignin-modified phenolic resin and metal borate in the preparation of plywood, and adding modified alumina and fatty alcohol to the adhesive, the problems of high free formaldehyde content and insufficient bonding strength of existing plywood are solved. Improved corrosion resistance and bonding strength, extending service life.

CN115741908BActive Publication Date: 2024-10-18GUANGDONG ORIENT GS HOUSING CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202211467994.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-22
Publication Date
2024-10-18
Estimated Expiration
2042-11-22

AI Technical Summary

Technical Problem

In the existing preparation method of corrosion-resistant plywood, the free formaldehyde content is high and the bonding strength is insufficient, which affects its corrosion resistance and service life.

Method used

Lignin-modified phenolic resin and metal borate are used as anti-corrosion liquid components, and lignin-modified phenolic resin, modified alumina and fatty alcohol are added to the adhesive, and plywood is prepared through vacuum impregnation and hot pressing.

Benefits of technology

Significantly improves the corrosion resistance and bonding strength of plywood, while reducing free formaldehyde content and extending service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003957160090000121
    Figure BDA0003957160090000121
Patent Text Reader

Abstract

The invention discloses a corrosion-resistant plywood, which comprises 3 to 5 layers of veneers, wherein the veneers are immersed in an antiseptic liquid, and then dried to obtain the antiseptic veneers; the antiseptic veneers are bonded by an adhesive; the antiseptic liquid comprises 32 to 38 parts of lignin-modified phenolic resin, 1.2 to 1.8 parts of metal borate, 55 to 65 parts of 1.5 to 3.5 wt% hydrochloric acid, and 2.8 to 4.2 parts of a curing agent by weight; the adhesive comprises 58 to 68 parts of lignin-modified phenolic resin, 3 to 8 parts of graphene oxide, 12 to 18 parts of modified alumina, 9 to 13 parts of fatty alcohol, and 5 to 7 parts of sodium dodecylbenzene sulfonate by weight. The plywood prepared by the invention has strong corrosion resistance, high bonding strength, and low free formaldehyde content.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of artificial boards, and in particular to a corrosion-resistant plywood and a preparation method thereof. Background Art

[0002] Plywood is a board material made by bonding veneers with adhesives. It is usually used as packaging material for airplanes, trains and buildings. In order to extend the service life of plywood, plywood needs to have good strength to avoid breakage during use. At the same time, since plywood is a wooden board, it is easily corroded by microorganisms, fungi and termites during long-term use and storage, causing the plywood to mold and discolor, affecting the toughness and strength of the plywood, and thus affecting the service life of the finished products made of plywood.

[0003] CN114474267A discloses a method for preparing corrosion-resistant plywood, which comprises the following steps: drying a plurality of veneers, immersing the veneers in an antiseptic liquid, vacuum impregnating the veneers and the antiseptic liquid, taking them out, and obtaining a primary treated board; the antiseptic liquid is composed of an antiseptic, a water-soluble phenolic resin, a curing agent, and water in a mass ratio of (0.4-0.6): (15-25): (1-1.5): (95-105); the antiseptic is any one of boric acid, borax, and disodium octaborate tetrahydrate; drying the obtained primary treated board to obtain a spare board, applying an adhesive on the spare board, bonding a plurality of spare boards to each other, and obtaining a composite board; and hot pressing and cutting the composite board to obtain the composite board. The adhesive is composed of chitosan, whey protein, a modifier and 1% glacial acetic acid solution in a mass ratio of (1-3): (3-5): (0.5-0.8): (15-25). However, the plywood preparation process has a high free formaldehyde content and insufficient bonding strength due to the presence of phenolic resin in the preservative solution.

[0004] In summary, after extensive searching by the applicant, it is found that there are at least problems in the art such as high free formaldehyde content and insufficient bonding strength of plywood. Therefore, it is necessary to develop or improve a corrosion-resistant plywood and a preparation method thereof. Summary of the invention

[0005] Based on this, in order to solve the problems of poor corrosion resistance, insufficient free formaldehyde content and bonding strength of plywood, the present invention provides a corrosion-resistant plywood and a preparation method thereof. The specific technical scheme is as follows:

[0006] A corrosion-resistant plywood comprising 3 to 5 layers of veneers, wherein the veneers are immersed in an anti-corrosion liquid and then dried to obtain the anti-corrosion resistant veneer;

[0007] The anti-corrosion veneers are bonded together by adhesive;

[0008] The antiseptic solution includes, by weight, 32 to 38 parts of lignin-modified phenolic resin, 1.2 to 1.8 parts of metal borate, 55 to 65 parts of hydrochloric acid, and 2.8 to 4.2 parts of curing agent;

[0009] The adhesive comprises, by weight, 58 to 68 parts of lignin-modified phenolic resin, 3 to 8 parts of graphene oxide, 12 to 18 parts of modified aluminum oxide, 9 to 13 parts of fatty alcohol and 5 to 7 parts of sodium dodecylbenzene sulfonate.

[0010] Furthermore, the mass percentage of the hydrochloric acid is 1.5-3.5wt%.

[0011] Furthermore, the metal borate is any one of modified barium metaborate, zinc borate and sodium perborate.

[0012] Furthermore, the curing agent is hexamethylenetetramine or melamine.

[0013] Furthermore, the fatty alcohol is any one of lauryl alcohol, octanol and myristyl alcohol.

[0014] Furthermore, the preparation method of the lignin-modified phenolic resin comprises the following steps:

[0015] Phenol, lignin, bagasse and sodium alginate are added into a reactor and reacted at a constant temperature of 160 to 180°C and a reactor pressure of 2.5 to 2.8 MPa for 8 to 9 hours to obtain an intermediate reaction liquid;

[0016] Add oxalic acid and formaldehyde to the intermediate reaction solution in sequence, and react with constant temperature stirring for 3 to 3.6 hours, the reaction temperature is 82 to 92° C., and the stirring speed is 500 to 560 r / min to obtain a product;

[0017] The product is washed with water, and then dehydrated and dried to obtain the lignin-modified phenolic resin.

[0018] Furthermore, the preparation method of the modified alumina comprises the following steps:

[0019] Alumina is dispersed in anhydrous ethanol, and then phenyltriethoxysilane and hexadecyltrimethoxysilane are added, and stirred at room temperature for 6 to 8 hours at a stirring speed of 820 to 880 r / min to obtain the modified alumina after precipitation.

[0020] Furthermore, the single board is any one of poplar, basswood and fir.

[0021] The technical solution also provides a method for preparing plywood, which comprises the following steps:

[0022] Preparation of the antiseptic liquid: by weight, 32 to 38 parts of lignin-modified phenolic resin, 1.2 to 1.8 parts of metal borate, and 55 to 65 parts of 1.5 to 3.5 wt % hydrochloric acid are mixed uniformly, stirred for 25 to 30 minutes, and then 2.8 to 4.2 parts of a curing agent are added, and stirred at 35 to 38° C. for 46 to 52 minutes to obtain the antiseptic liquid;

[0023] Preparation of the adhesive: by weight, 58 to 68 parts of lignin-modified phenolic resin, 3 to 8 parts of graphene oxide, 12 to 18 parts of modified alumina, 9 to 13 parts of fatty alcohol and 5 to 7 parts of sodium dodecylbenzene sulfonate are uniformly mixed, and stirred at 42 to 48° C. for 95 to 115 minutes to obtain the adhesive;

[0024] Cleaning 3 to 5 layers of veneer and then vacuum drying them, and then vacuum injecting and dipping them with the anti-corrosion liquid, and drying them to obtain the anti-corrosion resistant veneer;

[0025] Glue is evenly applied on the surface of the anti-corrosion veneer, and the glued surfaces of the anti-corrosion veneer are bonded to each other to obtain the plywood.

[0026] Furthermore, the vacuum drying conditions are: vacuum degree -0.05 to -0.08 MPa, temperature 60 to 65°C;

[0027] The vacuum injection impregnation treatment conditions are as follows: firstly, the vacuum dried veneer is placed in a vacuum pressure tank, evacuated to -0.06 to -0.09 MPa, maintained for 25 to 30 minutes, then the preservative liquid is added to the vacuum pressure tank, pressurized to 1.8 to 2.6 MPa, maintained for 50 to 55 minutes, and then the pressure is released;

[0028] The drying process is carried out under the following conditions: temperature 115-120°C.

[0029] Furthermore, the amount of glue on the surface of the anti-corrosion veneer is 260-320 g / m 2 .

[0030] In the above technical scheme, since the antiseptic liquid adopts lignin-modified phenolic resin and metal borate, and the adhesive adopts lignin-modified phenolic resin, modified alumina and fatty alcohol, the prepared plywood has strong corrosion resistance, high bonding strength and low free formaldehyde content. Specifically, the antiseptic liquid and the adhesive contain lignin-modified phenolic resin at the same time, and have a specific effect with other ingredients, which can significantly improve the corrosion resistance of the plywood and reduce the free formaldehyde content. The veneer is immersed in the antiseptic liquid containing lignin-modified phenolic resin and metal borate, which can strengthen the corrosion resistance of the veneer; the lignin-modified phenolic resin can better fix free formaldehyde, so the corrosion-resistant veneer of the present invention has a low free formaldehyde content. The corrosion-resistant veneers are bonded together with adhesives. On the one hand, the fatty alcohol contained in the adhesive can significantly improve the bonding strength of the plywood when reacting with other ingredients, especially lignin-modified phenolic resin and modified alumina; on the other hand, the lignin-modified phenolic resin contained in the adhesive can reduce the overall free formaldehyde content of the plywood. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with its embodiments. It should be understood that the specific implementation methods described herein are only used to explain the present invention and do not limit the protection scope of the present invention.

[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0033] A corrosion-resistant plywood in one embodiment of the present invention comprises 3 to 5 layers of veneers, wherein the veneers are immersed in an anti-corrosion liquid and then dried to obtain the anti-corrosion resistant veneer;

[0034] The anti-corrosion veneers are bonded together by adhesive;

[0035] The antiseptic solution includes, by weight, 32 to 38 parts of lignin-modified phenolic resin, 1.2 to 1.8 parts of metal borate, 55 to 65 parts of hydrochloric acid, and 2.8 to 4.2 parts of curing agent;

[0036] The adhesive comprises, by weight, 58 to 68 parts of lignin-modified phenolic resin, 3 to 8 parts of graphene oxide, 12 to 18 parts of modified aluminum oxide, 9 to 13 parts of fatty alcohol and 5 to 7 parts of sodium dodecylbenzene sulfonate.

[0037] In one of the embodiments, the mass percentage of the hydrochloric acid is 1.5-3.5wt%.

[0038] In one embodiment, the metal borate is any one of modified barium metaborate, zinc borate and sodium perborate. Preferably, the metal borate is modified barium metaborate or zinc borate. Further preferably, the metal borate is modified barium metaborate.

[0039] In one embodiment, the curing agent is hexamethylenetetramine or melamine.

[0040] In one embodiment, the fatty alcohol is any one of lauryl alcohol, octanol and myristyl alcohol. Preferably, the fatty alcohol is lauryl alcohol or octanol. Further preferably, the fatty alcohol is lauryl alcohol.

[0041] In one embodiment, the preparation method of the lignin-modified phenolic resin comprises the following steps:

[0042] Phenol, lignin, bagasse and sodium alginate are added into a reactor and reacted at a constant temperature of 160 to 180°C and a reactor pressure of 2.5 to 2.8 MPa for 8 to 9 hours to obtain an intermediate reaction liquid;

[0043] Add oxalic acid and formaldehyde to the intermediate reaction solution in sequence, and react with constant temperature stirring for 3 to 3.6 hours, the reaction temperature is 82 to 92° C., and the stirring speed is 500 to 560 r / min to obtain a product;

[0044] The product is washed with water, and then dehydrated and dried to obtain the lignin-modified phenolic resin.

[0045] In one embodiment, the method for preparing the modified alumina comprises the following steps:

[0046] Alumina is dispersed in anhydrous ethanol, and then phenyltriethoxysilane and hexadecyltrimethoxysilane are added, and stirred at room temperature for 6 to 8 hours at a stirring speed of 820 to 880 r / min to obtain the modified alumina after precipitation.

[0047] In one embodiment, the veneer is any one of poplar, basswood and fir. Preferably, the veneer is poplar or basswood. More preferably, the veneer is poplar.

[0048] In one embodiment, the technical solution provides a method for preparing plywood, which comprises the following steps:

[0049] Preparation of the antiseptic liquid: by weight, 32 to 38 parts of lignin-modified phenolic resin, 1.2 to 1.8 parts of metal borate, and 55 to 65 parts of 1.5 to 3.5 wt % hydrochloric acid are mixed uniformly, stirred for 25 to 30 minutes, and then 2.8 to 4.2 parts of a curing agent are added, and stirred at 35 to 38° C. for 46 to 52 minutes to obtain the antiseptic liquid;

[0050] Preparation of the adhesive: by weight, 58 to 68 parts of lignin-modified phenolic resin, 3 to 8 parts of graphene oxide, 12 to 18 parts of modified alumina, 9 to 13 parts of fatty alcohol and 5 to 7 parts of sodium dodecylbenzene sulfonate are uniformly mixed, and stirred at 42 to 48° C. for 95 to 115 minutes to obtain the adhesive;

[0051] Cleaning 3 to 5 layers of veneer and then vacuum drying them, and then vacuum injecting and dipping them with the anti-corrosion liquid, and drying them to obtain the anti-corrosion resistant veneer;

[0052] Glue is evenly applied on the surface of the anti-corrosion veneer, and the glued surfaces of the anti-corrosion veneer are bonded to each other to obtain the plywood.

[0053] In one embodiment, the vacuum drying conditions are: vacuum degree -0.05 to -0.08 MPa, temperature 60 to 65°C;

[0054] The vacuum injection impregnation treatment conditions are as follows: firstly, the vacuum dried veneer is placed in a vacuum pressure tank, evacuated to -0.06 to -0.09 MPa, maintained for 25 to 30 minutes, then the preservative liquid is added to the vacuum pressure tank, pressurized to 1.8 to 2.6 MPa, maintained for 50 to 55 minutes, and then the pressure is released;

[0055] The drying process is carried out under the following conditions: temperature 115-120°C.

[0056] Preferably, the vacuum drying conditions are: vacuum degree -0.06 to -0.08 MPa, temperature 62 to 65°C;

[0057] The vacuum injection impregnation treatment conditions are as follows: firstly, the vacuum-dried veneer is placed in a vacuum pressure tank, evacuated to -0.07 to -0.09 MPa, and maintained for 26 to 30 minutes, then the preservative liquid is added to the vacuum pressure tank, pressurized to 2.0 to 2.6 MPa, maintained for 51 to 55 minutes, and then the pressure is released;

[0058] The drying process is carried out under the following conditions: temperature 116-120°C.

[0059] Further preferably, the vacuum drying conditions are: vacuum degree -0.06 to -0.07 MPa, temperature 62 to 63°C;

[0060] The vacuum injection impregnation treatment conditions are as follows: firstly, the vacuum dried veneer is placed in a vacuum pressure tank, evacuated to -0.07-0.08 MPa, maintained for 26-28 minutes, then the preservative liquid is added to the vacuum pressure tank, pressurized to 2.0-2.3 MPa, maintained for 52-53 minutes, and then the pressure is released;

[0061] The drying process is carried out under the following conditions: temperature of 116-119°C.

[0062] In one embodiment, the amount of glue on the surface of the anti-corrosion veneer is 260-320 g / m 2 Preferably, the amount of adhesive on the surface of the anti-corrosion veneer is 270-320 g / m 2 Preferably, the amount of adhesive on the surface of the anti-corrosion veneer is 270-310 g / m 2 .

[0063] The embodiments of the present invention will be described in detail below with reference to specific examples.

[0064] Embodiment 1:

[0065] Preparation of lignin-modified phenolic resin: Phenol, lignin, bagasse and sodium alginate are added to a reactor, and the reaction is carried out at a constant temperature of 170°C for 8.5 hours, and the reactor pressure is 2.7MPa to obtain an intermediate reaction liquid; oxalic acid and formaldehyde are added to the intermediate reaction liquid in sequence, and the reaction is stirred at a constant temperature of 87°C for 3.3 hours, and the stirring speed is 530r / min to obtain a product; the product is washed with water, and then dehydrated and dried to obtain a lignin-modified phenolic resin.

[0066] Preparation of modified alumina: Alumina was dispersed in anhydrous ethanol, and then phenyltriethoxysilane and hexadecyltrimethoxysilane were added, stirred at room temperature for 7 hours at a stirring speed of 850 r / min, and modified alumina was obtained after precipitation.

[0067] Preparation of preservative liquid: By mass, 35 parts of lignin modified phenolic resin, 1.5 parts of modified barium metaborate, and 60 parts of 2.5wt% hydrochloric acid were mixed evenly, stirred for 28 minutes, and then 3.5 parts of hexamethylenetetramine were added, and stirred at 37°C for 49 minutes to obtain a preservative liquid.

[0068] Preparation of adhesive: 63 parts by weight of lignin-modified phenolic resin, 5 parts by weight of graphene oxide, 15 parts by weight of modified alumina, 11 parts by weight of lauryl alcohol and 6 parts by weight of sodium dodecylbenzene sulfonate were mixed uniformly, and stirred at 45° C. for 105 min to obtain an adhesive;

[0069] After washing the four layers of poplar wood, vacuum drying was performed at a vacuum degree of -0.07 MPa and a temperature of 63°C. The vacuum-dried poplar wood was then placed in a vacuum pressure tank, evacuated to -0.08 MPa, and maintained for 27 minutes. The preservative liquid was added to the vacuum pressure tank, pressurized to 2.2 MPa, maintained for 53 minutes, and depressurized. After drying at 118°C, the antiseptic poplar wood was obtained. Glue was evenly applied on the surface of the antiseptic poplar wood, and the amount of glue applied was 290 g / m 2 , the cloth glue surfaces of the antiseptic poplar wood are bonded to each other to obtain plywood.

[0070] Embodiment 2:

[0071] The other parts are the same as those in Example 1, except that the modified barium metaborate is replaced by zinc borate.

[0072] Embodiment 3:

[0073] The other parts are the same as those in Example 1, except that the modified barium metaborate is replaced by sodium perborate.

[0074] Embodiment 4:

[0075] The other parts are the same as those in Example 1, except that hexamethylenetetramine is replaced by melamine.

[0076] Embodiment 5:

[0077] The other parts are the same as those in Example 1, except that lauryl alcohol is replaced by octanol.

[0078] Embodiment 6:

[0079] The other parts are the same as those in Example 1, except that lauryl alcohol is replaced by myristyl alcohol.

[0080] Embodiment 7:

[0081] The other parts are the same as those in Example 1, except that poplar wood is replaced by basswood.

[0082] Comparative Example 1:

[0083] Preparation of modified alumina: Alumina was dispersed in anhydrous ethanol, and then phenyltriethoxysilane and hexadecyltrimethoxysilane were added, stirred at room temperature for 7 hours at a stirring speed of 850 r / min, and modified alumina was obtained after precipitation.

[0084] Preparation of antiseptic liquid: By mass, 35 parts of phenolic resin, 1.5 parts of modified barium metaborate, and 60 parts of 2.5wt% hydrochloric acid were mixed evenly, stirred for 28 minutes, and then 3.5 parts of hexamethylenetetramine were added, and stirred at 37°C for 49 minutes to obtain the antiseptic liquid.

[0085] Preparation of adhesive: 63 parts of phenolic resin, 5 parts of graphene oxide, 15 parts of modified alumina, 11 parts of lauryl alcohol and 6 parts of sodium dodecylbenzene sulfonate were mixed uniformly by weight, and stirred at 45° C. for 105 min to obtain an adhesive;

[0086] After washing the four layers of poplar wood, vacuum drying was performed at a vacuum degree of -0.07 MPa and a temperature of 63°C. The vacuum-dried poplar wood was then placed in a vacuum pressure tank, evacuated to -0.08 MPa, and maintained for 27 minutes. The preservative liquid was added to the vacuum pressure tank, pressurized to 2.2 MPa, maintained for 53 minutes, and depressurized. After drying at 118°C, the antiseptic poplar wood was obtained. Glue was evenly applied on the surface of the antiseptic poplar wood, and the amount of glue applied was 290 g / m 2 , the cloth glue surfaces of the antiseptic poplar wood are bonded to each other to obtain plywood.

[0087] Comparative Example 2:

[0088] Preparation of lignin-modified phenolic resin: Phenol, lignin, bagasse and sodium alginate are added to a reactor, and the reaction is carried out at a constant temperature of 170°C for 8.5 hours, and the reactor pressure is 2.7MPa to obtain an intermediate reaction liquid; oxalic acid and formaldehyde are added to the intermediate reaction liquid in sequence, and the reaction is stirred at a constant temperature of 87°C for 3.3 hours, and the stirring speed is 530r / min to obtain a product; the product is washed with water, and then dehydrated and dried to obtain a lignin-modified phenolic resin.

[0089] Preparation of modified alumina: Alumina was dispersed in anhydrous ethanol, and then phenyltriethoxysilane and hexadecyltrimethoxysilane were added, stirred at room temperature for 7 hours at a stirring speed of 850 r / min, and modified alumina was obtained after precipitation.

[0090] Preparation of the preservative liquid: By mass, 35 parts of lignin-modified phenolic resin, 1.5 parts of boric acid, and 60 parts of 2.5wt% hydrochloric acid were mixed evenly, stirred for 28 minutes, and then 3.5 parts of hexamethylenetetramine were added, and stirred at 37°C for 49 minutes to obtain the preservative liquid.

[0091] Preparation of adhesive: 63 parts by weight of lignin-modified phenolic resin, 5 parts by weight of graphene oxide, 15 parts by weight of modified alumina, 11 parts by weight of lauryl alcohol and 6 parts by weight of sodium dodecylbenzene sulfonate were mixed uniformly, and stirred at 45° C. for 105 min to obtain an adhesive;

[0092] After cleaning the 4 layers of poplar wood, vacuum dry them at a vacuum degree of -0.07MPa and a temperature of 63°C, then place the vacuum-dried poplar wood in a vacuum pressure tank, evacuate to -0.08MPa, and keep it for 27 minutes, add the preservative liquid into the vacuum pressure tank, pressurize it to 2.2MPa, keep it for 53 minutes, release the pressure, and dry it at 118°C to obtain the anti-corrosion poplar wood; evenly apply glue on the surface of the anti-corrosion poplar wood, the glue amount is 290g / m2, and the glued surfaces of the anti-corrosion poplar wood are bonded to each other to obtain plywood.

[0093] Comparative Example 3:

[0094] Preparation of lignin-modified phenolic resin: Phenol, lignin, bagasse and sodium alginate are added to a reactor, and the reaction is carried out at a constant temperature of 170°C for 8.5 hours, and the reactor pressure is 2.7MPa to obtain an intermediate reaction liquid; oxalic acid and formaldehyde are added to the intermediate reaction liquid in sequence, and the reaction is stirred at a constant temperature of 87°C for 3.3 hours, and the stirring speed is 530r / min to obtain a product; the product is washed with water, and then dehydrated and dried to obtain a lignin-modified phenolic resin.

[0095] Preparation of preservative liquid: By mass, 35 parts of lignin modified phenolic resin, 1.5 parts of modified barium metaborate, and 60 parts of 2.5wt% hydrochloric acid were mixed evenly, stirred for 28 minutes, and then 3.5 parts of hexamethylenetetramine were added, and stirred at 37°C for 49 minutes to obtain a preservative liquid.

[0096] Preparation of adhesive: 63 parts by weight of lignin-modified phenolic resin, 5 parts of graphene oxide, 15 parts of aluminum oxide, 11 parts of lauryl alcohol and 6 parts of sodium dodecylbenzene sulfonate were mixed uniformly, and stirred at 45° C. for 105 min to obtain an adhesive;

[0097] After cleaning the 4 layers of poplar wood, vacuum dry them at a vacuum degree of -0.07MPa and a temperature of 63°C, then place the vacuum-dried poplar wood in a vacuum pressure tank, evacuate to -0.08MPa, and keep it for 27 minutes, add the preservative liquid into the vacuum pressure tank, pressurize it to 2.2MPa, keep it for 53 minutes, release the pressure, and dry it at 118°C to obtain the anti-corrosion poplar wood; evenly apply glue on the surface of the anti-corrosion poplar wood, the glue amount is 290g / m2, and the glued surfaces of the anti-corrosion poplar wood are bonded to each other to obtain plywood.

[0098] Comparative Example 4:

[0099] Preparation of lignin-modified phenolic resin: Phenol, lignin, bagasse and sodium alginate are added to a reactor, and the reaction is carried out at a constant temperature of 170°C for 8.5 hours, and the reactor pressure is 2.7MPa to obtain an intermediate reaction liquid; oxalic acid and formaldehyde are added to the intermediate reaction liquid in sequence, and the reaction is stirred at a constant temperature of 87°C for 3.3 hours, and the stirring speed is 530r / min to obtain a product; the product is washed with water, and then dehydrated and dried to obtain a lignin-modified phenolic resin.

[0100] Preparation of modified alumina: Alumina was dispersed in anhydrous ethanol, and then phenyltriethoxysilane and hexadecyltrimethoxysilane were added, stirred at room temperature for 7 hours at a stirring speed of 850 r / min, and modified alumina was obtained after precipitation.

[0101] Preparation of preservative liquid: By mass, 35 parts of lignin modified phenolic resin, 1.5 parts of modified barium metaborate, and 60 parts of 2.5wt% hydrochloric acid were mixed evenly, stirred for 28 minutes, and then 3.5 parts of hexamethylenetetramine were added, and stirred at 37°C for 49 minutes to obtain a preservative liquid.

[0102] Preparation of adhesive: 63 parts by weight of lignin-modified phenolic resin, 5 parts of graphene oxide, 15 parts of modified alumina, 11 parts of ethanol and 6 parts of sodium dodecylbenzene sulfonate were mixed uniformly, and stirred at 45° C. for 105 min to obtain an adhesive;

[0103] After cleaning the 4 layers of poplar wood, vacuum dry them at a vacuum degree of -0.07MPa and a temperature of 63°C, then place the vacuum-dried poplar wood in a vacuum pressure tank, evacuate to -0.08MPa, and keep it for 27 minutes, add the preservative liquid into the vacuum pressure tank, pressurize it to 2.2MPa, keep it for 53 minutes, release the pressure, and dry it at 118°C to obtain the anti-corrosion poplar wood; evenly apply glue on the surface of the anti-corrosion poplar wood, the glue amount is 290g / m2, and the glued surfaces of the anti-corrosion poplar wood are bonded to each other to obtain plywood.

[0104] Test Method

[0105] Anti-corrosion performance test method: Test according to LY / T12832011 and judge by the mass loss rate of the test sample.

[0106] Bonding strength test method: Test according to GB / T18102-2000.

[0107] Free formaldehyde test method: Test according to GB / T 17657-2013.

[0108] The plywood of Examples 1 to 7 and Comparative Examples 1 to 4 were subjected to relevant performance tests, and the test results are shown in Table 1.

[0109] Table 1:

[0110]

[0111]

[0112] As can be seen from Table 1, since the antiseptic liquid of the present invention adopts lignin-modified phenolic resin and metal borate, and its adhesive adopts lignin-modified phenolic resin, modified alumina and fatty alcohol, the prepared plywood has strong corrosion resistance, high bonding strength and low free formaldehyde content.

[0113] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0114] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A corrosion-resistant plywood, characterized in that: It comprises 3 to 5 layers of veneers, which are immersed in an antiseptic liquid and then dried to obtain an antiseptic veneer; The anti-corrosion veneers are bonded together by adhesive; The antiseptic solution comprises, by weight, 32 to 38 parts of lignin-modified phenolic resin, 1.2 to 1.8 parts of metal borate, 55 to 65 parts of 1.5 to 3.5 wt % hydrochloric acid, and 2.8 to 4.2 parts of a curing agent; The adhesive comprises, by weight, 58 to 68 parts of lignin-modified phenolic resin, 3 to 8 parts of graphene oxide, 12 to 18 parts of modified alumina, 9 to 13 parts of fatty alcohol and 5 to 7 parts of sodium dodecylbenzene sulfonate; The preparation method of the lignin-modified phenolic resin comprises the following steps: Phenol, lignin, bagasse and sodium alginate are added into a reactor and reacted at a constant temperature of 160 to 180°C and a reactor pressure of 2.5 to 2.8 MPa for 8 to 9 hours to obtain an intermediate reaction liquid; Add oxalic acid and formaldehyde to the intermediate reaction solution in sequence, and react with constant temperature stirring for 3 to 3.6 hours, the reaction temperature is 82 to 92° C., and the stirring speed is 500 to 560 r / min to obtain a product; Washing the product with water, and then dehydrating and drying it to obtain the lignin-modified phenolic resin; The preparation method of the modified alumina comprises the following steps: Alumina is dispersed in anhydrous ethanol, and then phenyltriethoxysilane and hexadecyltrimethoxysilane are added, and stirred at room temperature for 6 to 8 hours at a stirring speed of 820 to 880 r / min to obtain the modified alumina after precipitation.

2. The plywood according to claim 1, characterized in that: The metal borate is any one of modified barium metaborate, zinc borate and sodium perborate.

3. The plywood according to claim 1, characterized in that: The curing agent is hexamethylenetetramine or melamine.

4. The plywood according to claim 1, characterized in that: The fatty alcohol is any one of lauryl alcohol, octanol and myristyl alcohol.

5. The plywood according to claim 1, characterized in that: The veneer is any one of poplar, basswood and fir.

6. The method for preparing plywood according to any one of claims 1 to 5, characterized in that: It includes the following steps: Preparation of the antiseptic liquid: by weight, 32 to 38 parts of lignin-modified phenolic resin, 1.2 to 1.8 parts of metal borate, and 55 to 65 parts of 1.5 to 3.5 wt % hydrochloric acid are mixed uniformly, stirred for 25 to 30 minutes, and then 2.8 to 4.2 parts of a curing agent are added, and stirred at 35 to 38° C. for 46 to 52 minutes to obtain the antiseptic liquid; Preparation of the adhesive: by weight, 58 to 68 parts of lignin-modified phenolic resin, 3 to 8 parts of graphene oxide, 12 to 18 parts of modified alumina, 9 to 13 parts of fatty alcohol and 5 to 7 parts of sodium dodecylbenzene sulfonate are uniformly mixed, and stirred at 42 to 48° C. for 95 to 115 minutes to obtain the adhesive; Cleaning 3 to 5 layers of veneer and then vacuum drying them, and then vacuum injecting and dipping them with the anti-corrosion liquid, and drying them to obtain the anti-corrosion resistant veneer; Glue is evenly applied on the surface of the anti-corrosion veneer, and the glued surfaces of the anti-corrosion veneer are bonded to each other to obtain the plywood.

7. The preparation method according to claim 6, characterized in that: The vacuum drying conditions are: vacuum degree -0.05 to -0.08 MPa, temperature 60 to 65°C; The vacuum injection impregnation treatment conditions are as follows: firstly, the vacuum dried veneer is placed in a vacuum pressure tank, evacuated to -0.06 to -0.09 MPa, maintained for 25 to 30 minutes, then the preservative liquid is added to the vacuum pressure tank, pressurized to 1.8 to 2.6 MPa, maintained for 50 to 55 minutes, and then the pressure is released; The drying process is carried out under the following conditions: temperature 115-120°C.

8. The preparation method according to claim 6, characterized in that: The amount of glue on the surface of the anti-corrosion veneer is 260-320g / m 2 .

Citation Information

Patent Citations

  • Corrosion-resistant plywood and preparation method thereof

    CN114474267A

  • Laminate, preparation method for laminate and application of laminate

    CN103568081A

  • Preparation method of waterproof daub with high bonding strength

    CN109336463A

  • Composite material modified wear-resistant and corrosion-resistant coating as well as preparation method thereof

    CN110527404A

  • Bamboo building curtain wall panel and preparation method thereof

    CN111379362A