A kind of polyester antistatic release film and its production method
Through the design of polyester composite film structure and adhesive release layer, the problems of uneven coating and electrostatic adsorption of PET release film are solved, and a stable release, environmentally friendly and high-performance polyester antistatic release film is achieved. Solvent contamination and high-cost production are avoided.
Patent Information
- Application Number
- CN202211487396.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-25
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-11-25
AI Technical Summary
Existing PET release films make loud noises when peeled off, are coated unevenly, and electrostatically adsorb dust, and fluorine release agents require a large amount of solvents, resulting in production hazards and high costs.
The polyester composite film structure is adopted, including antistatic PET film and PET porous film, and a three-layer structure is prepared by coating with an adhesive release layer. No release agent is coated on the surface of the film, and polytrifluoropropylmethyl silicone is used. Oxane is cross-linked with methyl silicate to form a network structure, which is combined with wax emulsion and water-based polyurethane curing agent to form a uniformly dispersed release layer in the pores to reduce adhesion.
It achieves stable release effect, green environmental protection, high tensile strength and tearing strength, clean surface and no scratches, improves the problem of silicone oil residue and solvent pollution, and improves stiffness, heat resistance and flatness.
Smart Images

Figure CN115742374B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of antistatic release films, and in particular relates to a polyester antistatic release film and a production method thereof. Background Art
[0002] PET release film is a material commonly used in thermal transfer. The base material is PET, which is coated with silicone oil, so it is also called silicone oil film. PET release film is now widely used in packaging, printing, silk screen, pad printing, nameplate, membrane switch, flexible circuit, insulation products, circuit board, laser anti-counterfeiting, lamination, electronics, sealing material film, reflective material, waterproof material, medicine, sanitary paper, adhesive products, die-cutting and other industries. The sound when peeling off is caused by excessive release force and uneven coating. It cannot be peeled off after being pasted with the tape. It is generally caused by uneven coating. Some release films have serious leakage, which will make a certain part have no release effect, making the tape unable to be peeled off. The greasy release surface is mainly caused by the release agent system. It is not that greasy things are necessarily bad. In fact, some greasy release films have a more uniform surface coating and a better residual adhesion rate. But some are purely poor in adhesion, and the silicone oil is easy to fall off. Release film will generate static electricity and absorb dust during the unwinding and rewinding process. Condensation-type silicone release agents were first industrialized in 1954. Addition-type silicone release agents were first industrialized in 1975. They are mainly dimethyl polysiloxane with vinyl groups, which react with crosslinking agents containing silicon-hydrogen bonds under the catalysis of metal platinum compounds to undergo silylation reaction and crosslinking and curing. Fluorine release agents are cured by thermal curing. The oven length is long. All fluorine release agents on the market are low-viscosity and have poor leveling. Fluorine release agents require the addition of a large amount of solvent to assist leveling. Rainbow lines, crystal points and other problems are all improved and adjusted with solvents. In addition, the trough life of the release agent and the curing efficiency of the film can also be appropriately adjusted by solvents. Some fluorine release agents on the market must be diluted with fluorine-containing solvents. A single solvent is not enough, and a mixed solvent is required. Use a strong solvent to thoroughly dissolve the fluorine release agent, and then add some solvents with good wettability to the substrate to assist leveling and adjust the volatilization rate. There are solvent hazards during production, and the production price is high. As a person skilled in the art, it is urgent to develop a new polyester antistatic release film and a production method thereof. Summary of the invention
[0003] The purpose of the present invention is to provide a polyester antistatic release film and a production method thereof in view of the existing problems. The present invention does not coat a release agent on the surface of the film.
[0004] The present invention is achieved through the following technical solutions:
[0005] A polyester antistatic release film comprises a polyester composite film, wherein the surface of the polyester composite film is not provided with a release agent, the polyester composite film comprises an inner layer, an adhesive release layer, and an outer layer, wherein the inner layer is an antistatic PET film, and the outer layer is a PET porous film. The polyester composite film is a three-layer structure prepared by coating and compounding the adhesive release layer, and has a thickness of 25 to 150 microns. The production method of the polyester composite film comprises the following steps: (1) corona treatment on the surface of the inner PET film; (2) coating the adhesive release layer: the antistatic PET film is subjected to an unwinding tension of 40 to 60 N and a coating pressure of 2.5 to 3 kg / cm 2 , coating amount 2.5-3.5g / m 2 , the temperature of the pressure roller is 70~75℃, and the antistatic PET film coated with glue is obtained; (3) drying; (4) compounding: the dried antistatic PET film coated with glue is compounded by coating with an adhesive release layer; (5) winding and aging: the winding speed is 130~150m / min, the winding tension is 140~170N, and after winding, it is aged for 36~48h at a temperature of 40~50℃ and a relative humidity of 50~75%.
[0006] Furthermore, the adhesive release layer is prepared by mixing 25-30% alcohol-soluble polyurethane, 2-3% polytrifluoropropylmethylsiloxane, 5-7% wax emulsion and industrial alcohol in percentage, then adding 1-2% methyl silicate, and finally adding a cross-linking agent, and mixing evenly to obtain an adhesive release layer with a solid content of 20%-35%, wherein the cross-linking agent is a mixture of organic tin and water-based polyurethane curing agent in a mass ratio of 1:1, the organic tin is dibutyltin dilaurate or dibutyltin dilaurate, and the water-based polyurethane curing agent is Aquolin270 or Aquolin278, and the wax emulsion is prepared by heating hydrogenated castor oil to 90-95°C, then adding 4-6% of sodium dodecyl sulfate by mass of hydrogenated castor oil, and fully mechanically stirring at 3000rpm to disperse and emulsify it to obtain a wax emulsion with a solid content of 10-12%.
[0007] Furthermore, the drying temperature in step (3) is 95-120° C., and the drying time is 2-3 s.
[0008] Furthermore, the PET porous film has a pore size of 2-5 μm and a film thickness of 25-40 μm.
[0009] Furthermore, in the step (4), the compounding pressure is 0.1-0.2 MPa, the compounding speed is 130-150 m / min, the pulling pressure is 3-5 kg / cm2, the preheating temperature is 40-50°C, the compounding temperature is 60-70°C, the cooling temperature is 15°C, and the unwinding tension of the PET porous film is 80-110 N.
[0010] Furthermore, in the step (1), the corona treatment voltage is 10-20 kV, the frequency is 10-25 kHz, the electrode spacing is 1-2 mm, and the surface tension of the inner PET film after corona treatment reaches 45-50 mN / m.
[0011] Beneficial effects of the present invention:
[0012] The production method of the polyester antistatic release film disclosed in the present invention does not coat a release agent on the surface of the film, but adopts an adhesive release layer with dual functions, one of which is an outer PET porous film and an inner antistatic PET film, and the adhesive release layer is used as an adhesive to make the two coated and composited, and after aging, the release component of the adhesive release layer as the middle layer of the release film enters the pores of the PET porous film to form a release effect, and the size of the release force can be obtained by adjusting the PET porous films with different pore sizes. The preparation method is simple, wherein polytrifluoropropylmethylsiloxane and methyl silicate can undergo dealcoholization reaction, the molecular structure of methyl silicate can make polytrifluoropropylmethylsiloxane form a network cross-linked structure, and the curing agent It can crosslink and solidify the polyurethane resin, and further improve the release ability to generate a low surface energy material with excellent mechanical strength. The adhesive release layer contains polytrifluoropropylmethylsiloxane and wax emulsion, which are miscible with the adhesive release layer in the presence of alcohol. After aging for 36 to 48 hours at a temperature of 40 to 50°C and a relative humidity of 50 to 75%, the ethanol evaporates, making the polytrifluoropropylmethylsiloxane and castor wax incompatible with the polyurethane resin itself. They slowly migrate from the inside of the polyurethane adhesive to the inside of the PET porous film, forming a uniformly dispersed release layer in the pores, thereby reducing the force with the adhesive, so that the release film has no stickiness or slight stickiness after contact with specific materials under limited conditions, achieving the release effect. 1
[0013] Compared with the prior art, the present invention has the following advantages:
[0014] The polyester antistatic release film disclosed in the present invention has stable release effect, is green and environmentally friendly, has high tensile strength and tear resistance, small shrinkage, high anti-adhesion force and other characteristics. The surface is clean and scratch-free, the coating is uniform, there is no transfer, and the shrinkage is small, which improves the previous silicone oil residual pollution problem and the solvent pollution problem of fluorine coating. The polyester antistatic release film has high stiffness and a smooth surface. Especially when it is used as a film substrate, it has good heat resistance and is suitable for high-temperature glue coating and dipped glue dust removal. It has good flatness, high cleanliness, high light transmittance, stable release effect and other functional characteristics. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 It is a schematic diagram of the structure of the polyester antistatic release film disclosed in the present invention, wherein 1 is the inner layer, 2 is the adhesive release layer, 3 is the outer layer, and 301-hole. DETAILED DESCRIPTION
[0016] The present invention is described below with specific examples, but is not intended to be limiting of the present invention. Example 1
[0017] A production method of polyester antistatic release film:
[0018] The polyester antistatic release film comprises a polyester composite film, the surface of the polyester composite film is not provided with a release agent, the polyester composite film comprises an inner layer, an adhesive release layer, and an outer layer, the inner layer is an antistatic PET film, the outer layer is a PET porous film with an average pore size of 5 μm, a porosity of 45%, and a film thickness of 25 μm, and the polyester composite film is a three-layer structure prepared by coating and compounding; the production method specifically comprises the following steps: (1) corona treatment on the surface of the inner PET film: the corona treatment voltage is 20 kV, the frequency is 25 kHz, the electrode spacing is 2 mm, and the surface tension reaches 50 mN / m; (2) coating the adhesive release layer: the inner PET film is unwound on the first unwinding device of the DLFHG1400C high-speed coating and compounding machine, the unwinding tension is 60 N, and the coating pressure is 3 kg / cm 2 , coating amount 3.5g / m 2 , roller temperature 75℃, pneumatic back pressure scraper; (3) Drying: drying temperature is 120℃; (4) Outer layer online lamination: lamination pressure 0.2MPa, lamination speed 150m / min, traction pressure 5kg / cm 2 The composite hot roller is Φ320mm, the surface is hard chrome plated and the oil medium is used for heat conduction, and the composite temperature is controlled at 70℃. The Φ320mm preheating roller is used for heat conduction and the constant temperature is controlled at 50℃. The cooling roller is Φ320mm and the water circulation cooling is at 15℃. The composite pressure roller is a Φ150mm rubber roller with a Shore hardness of 90A. The PET porous film is placed on the second unwinding device, and the unwinding tension is 110N. (5) Curling and aging: the winding speed tension is 170N, and the drying tunnel length of 16100 (L) × 4000 (W) × 5000 (H) mm is 12 meters. The aging temperature of the Tangpeiqi composite film aging room is 50℃ and the humidity is 75%, and the aging time is 48h.
[0019] The adhesive release layer is composed of 30% alcohol-soluble polyurethane and 3% polytrifluoropropylmethylsiloxane M by mass percentage. w2400, 7% wax emulsion and industrial alcohol are mixed evenly, and then 2% methyl silicate is added, and finally a cross-linking agent is added and mixed evenly to obtain an adhesive release layer with a solid content of 35%, wherein the cross-linking agent is a mixture of organic tin-dibutyltin dilaurate and Wanhua water-based polyurethane curing agent Aquolin278 in a mass ratio of 1:1, and the wax emulsion is hydrogenated castor oil wax heated to 95°C, and then sodium dodecyl sulfonate with a mass% of 6% of Haina Chemical Company's superior hydrogenated castor oil wax is added, and the wax emulsion with a solid content of 12% is obtained by fully mechanically stirring at 3000rpm for 30min to disperse and emulsify it. The preparation method of PET porous film refers to "Xi Peng, Wang Yan. Effective regulation and pore-forming process of porous structure on the surface of PET film [J]. Journal of Tianjin Polytechnic University, 2021, 40(03):10-14".
[0020] PET resin chips and 1% of the weight of the PET resin chips by weight of the polyli anti-WT4-4 static agent were put into a CHD-75 twin-screw extruder, and the barrel temperature was controlled in 9 sections at 180°C, 195°C, 210°C, 220°C, 230°C, 240°C, 250°C, 260°C, and 280°C. The main engine speed was 600r / min, and then mixed and extruded through a hanger die to form a cast sheet, which was then longitudinally stretched at a temperature of 80°C and a stretch ratio of 9; and transversely stretched at a temperature of 125°C and a stretch ratio of 8, and finally an antistatic PET film with a thickness of 40μm was prepared. Example 2
[0021] A production method of polyester antistatic release film:
[0022] The polyester antistatic release film comprises a polyester composite film, wherein the surface of the polyester composite film is not provided with a release agent, wherein the polyester composite film comprises an inner layer, an adhesive release layer, and an outer layer, wherein the outer layer is a PET porous film having an average pore size of 2 μm, a porosity of 50%, and a film thickness of 40 μm, and wherein the polyester composite film is a three-layer structure and is prepared by coating and compounding; the steps specifically comprising: (1) corona treatment on the surface of the inner PET film: the corona treatment voltage is 10 kV, the frequency is 10 kHz, the electrode spacing is 1 mm, and the surface tension reaches 45 mN / m; (2) coating the adhesive release layer: the inner PET film is unwound on the first unwinding device of a DLFHG1400C high-speed coating and compounding machine, the unwinding tension is 40 N, and the coating pressure is 2.5 kg / cm 2 , coating amount 2.5g / m 2, the pressure roller temperature is 75℃, and the scraper adopts a pneumatic back pressure scraper; (3) Drying: the drying temperature is 95℃, the time is 2s, and the air is blown; (4) Outer layer online compounding: compounding pressure 0.1MPa, compounding speed 150m / min, traction pressure 3kg / cm2; compounding hot roller Φ320mm, the surface is hard chrome plated, oil medium heat conduction, control the compounding temperature at 60℃, Φ320mm preheating roller oil medium heat conduction, constant temperature control 40℃, cooling roller Φ320mm, 15℃ water circulation cooling, compounding pressure roller Φ150mm Shore hardness 90A rubber roller, PET porous film is placed on the second unwinding device, and the unwinding tension is 80N; (5) Curling and aging: winding speed tension 140N, 16100L×4000W×5000Hmm drying tunnel with a length of 12 meters, aging temperature 40℃, humidity 50%, aging 36h.
[0023] The adhesive release layer is composed of 25% alcohol-soluble polyurethane and 2% polytrifluoropropylmethylsiloxane (QF-1) M w After 4600 and 5% wax emulsions are evenly mixed with industrial alcohol, 1% methyl silicate is added, and finally a cross-linking agent is added and mixed evenly to obtain an adhesive release layer with a solid content of 20%, wherein the cross-linking agent is a mixture of organic tin-dibutyltin dilaurate and Aquolin270 water-based polyurethane curing agent in a mass ratio of 1:1, and the wax emulsion is prepared by heating the superior hydrogenated castor oil wax of Haina Chemical Company to 90°C, and then adding 6% sodium dodecyl sulfate by mass of hydrogenated castor oil, and fully mechanically stirring at 3000rpm for 20min to disperse and emulsify it to obtain a wax emulsion with a solid content of 10%.
[0024] Among them, the antistatic PET resin chips CZ302 and the polyli anti-WT4-4 anti-static agent accounting for 1% of the mass of the PET resin chips were put into the CHD-75 twin-screw extruder, and the barrel temperature was controlled in 9 sections, and the temperature was controlled at 180℃, 195℃, 210℃, 220℃, 230℃, 240℃, 250℃, 260℃, and 280℃. The main engine speed was 500r / min, and the mixed extrusion was formed into a cast sheet through a hanger-type die head, and then longitudinally stretched at a temperature of 85℃ and a stretch ratio of 7; transversely stretched at a temperature of 130℃ and a stretch ratio of 6, and finally the sample was prepared with a thickness of 50μm.
[0025] The polyester antistatic release films of Examples 1 and 2 were subjected to performance tests, and the test results are shown in Table 1.
[0026] Table 1 Performance test results of polyester antistatic release films of Examples 1 to 2
[0027]
[0028] Note: The heat shrinkage rate shall be determined according to the test method specified in GB / T12027-2004; the transmittance and haze shall be determined according to the test method specified in GB / T2410-2008; the width and end surface uniformity shall be measured with the corresponding precision vernier ruler; the breaking strength and elongation shall be determined according to the test method specified in GB / T3923.1; the breakdown voltage shall be determined according to the test method specified in GB1408.1-2006; the appearance quality shall first visually inspect the quality of the film roll, and then sample 500mm from the full width of the end of the shafted film, and visually inspect the appearance quality of the sample film surface under the film viewing light. Thickness and thickness range: Take samples from the tail of the large axis film, starting from 30mm away from the edge of the film, grind the film horizontally to 3mm away from the other side, and use a thickness gauge with an accuracy of 1um to measure and record the thickness of all points measured at equal distances. The average value is the thickness of the axis, and the difference between the maximum thickness and the minimum thickness is recorded as the thickness range of the axis; paste the TESA7475 pressure-sensitive tape along the MD direction on the silicon-coated surface of the silicon-coated polyester film sample to be tested, cut it into a long strip sample of length × width = 175mm × 25.4mm according to the size of the tape, and roll the sample 3 times with a 2kg pressure wheel. Use FPT-F1 peel tester, peel at a peel angle of 180° and a speed of 300mm / min, and read the peel force data; the test method for thermal shrinkage rate shall be implemented in accordance with GB / T16958-2008.
Claims
1. A polyester antistatic release film, comprising a polyester composite film, characterized in that: The surface of the polyester composite film is not provided with a release agent. The polyester composite film includes an inner layer, an adhesive release layer, and an outer layer. The inner layer is an antistatic PET film, and the outer layer is a PET porous film. The polyester composite film is a three-layer structure prepared by coating and compounding the adhesive release layer, and the thickness is 25-150 microns; the adhesive release layer is prepared by mixing 25-30% alcohol-soluble polyurethane, 2-3% polytrifluoropropyl methylsiloxane, 5-7% wax emulsion and industrial alcohol in percentage, and then adding 1-2% methyl silicate, and finally adding a cross-linking agent, and mixing evenly to obtain an adhesive release layer with a solid content of 20%-35%, wherein the cross-linking agent is organic tin and water-based polyurethane curing agent. The wax emulsion is a mixture of an organic tin compound and an aqueous polyurethane curing agent in a mass ratio of 1:1, the organic tin compound is dibutyltin dilaurate or dibutyltin dilaurate, the aqueous polyurethane curing agent is Aquolin270 or Aquolin278, and the wax emulsion is prepared by heating hydrogenated castor oil to 90-95°C, then adding sodium dodecyl sulfate in an amount of 4-6% by mass of hydrogenated castor oil, and fully mechanically stirring at 3000 rpm for 20-30 minutes to obtain a wax emulsion with a solid content of 10-12%. The production method of the polyester composite film comprises the following steps: (1) corona treatment on the surface of the inner PET film; (2) coating an adhesive release layer: the antistatic PET film is subjected to a reeling tension of 40-60N and a coating pressure of 2.5-3kg / cm 2 , coating amount 2.5-3.5g / m 2 , the temperature of the pressure roller is 70~75℃, and the antistatic PET film coated with glue is obtained; (3) drying; (4) outer layer online compounding: the dried antistatic PET film coated with glue is compounded by coating with an adhesive release layer, and a PET porous membrane is placed on the second unwinding device; (5) winding and aging: the winding speed is 130~150m / min, the winding tension is 140~170N, and after winding, it is aged for 36~48h at a temperature of 40~50℃ and a relative humidity of 50~75%.
2. The polyester antistatic release film according to claim 1, characterized in that: The drying temperature in step (3) is 95-120° C. and the drying time is 2-3 seconds.
3. The polyester antistatic release film according to claim 1, characterized in that: The PET porous film has an average pore size of 2-5 μm, a film thickness of 25-40 μm, and a porosity of 40-50%.
4. The polyester antistatic release film according to claim 1, characterized in that: The compounding pressure of step (4) is 0.1-0.2 MPa, the compounding speed is 130-150 m / min, and the pulling pressure is 3-5 kg / cm 2 , preheating temperature 40~50℃, compounding temperature 60~70℃, cooling temperature 15℃, PET porous film unwinding tension is 80~110N.
5. The polyester antistatic release film according to claim 1, characterized in that: In the step (1), the corona treatment voltage is 10-20 kV, the frequency is 10-25 kHz, the electrode spacing is 1-2 mm, and the surface tension of the inner PET film after corona treatment reaches 45-50 mN / m.
Citation Information
Patent Citations
Coil stock-type local hot-melt double-sided adhesive tape
CN107868624A
Method for producing antistatic surface protective film, and antistatic surface protective film
CN112126372A