A composite retarder for magnesium phosphate cement-based materials and its application

By using a composite retarder of boric acid and additives in magnesium phosphate cement-based materials, the problem of poor retarding effect in the existing technology is solved, and the effects of extending the setting time, improving fluidity and enhancing strength are achieved, and is suitable for Quick fix project.

CN115745454BActive Publication Date: 2024-10-11UNIV OF JINAN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211655223.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-22
Publication Date
2024-10-11
Estimated Expiration
2042-12-22

AI Technical Summary

Technical Problem

The existing boric acid used as a retarder for magnesium phosphate cement-based materials cannot effectively delay the setting time, improve fluidity, and improve the strength of magnesium phosphate cement. There are problems such as insignificant retarding effect and early and late strength effects.

Method used

A magnesium phosphate cement-based material composite retarder including boric acid, triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate is used to extend the setting time, increase fluidity and improve the strength of magnesium phosphate cement by adjusting its mass ratio.

Benefits of technology

It effectively prolongs the setting time of magnesium phosphate cement, improves its fluidity and early strength, meets the needs of rapid repair projects, and at the same time improves the overall strength of the material to a certain extent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115745454B_ABST
    Figure CN115745454B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of cement retarders, and specifically relates to a composite retarder for magnesium phosphate cement-based materials and its application. The composite retarder for magnesium phosphate cement-based materials provided by the present invention comprises boric acid and an admixture; the admixture comprises the following raw materials: triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate; the mass ratio of the triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate is (80-90): (5-12): (1-5): (2-4). The present invention cooperates with boric acid, triethanolamine, aluminum nitrate, citric acid and polyphosphate to effectively prolong the setting time of magnesium phosphate cement-based materials, increase their fluidity, and also improve the strength of magnesium phosphate cement and its materials to a certain extent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cement retarders, and in particular relates to a magnesium phosphate cement-based material composite retarder and application thereof. Background Art

[0002] Acid-Base Cements (AB) appeared around the middle of the 19th century. Its basic principle is to generate corresponding salts through acid-base neutralization reaction between alkaline powder and acidic liquid to play a cementing role. Compared with traditional silicate cement, AB cement belongs to special cementitious materials. In general, as long as the alkaline oxide can react with the corresponding acidic liquid to generate salts, it can be used as the alkaline component of AB cement, such as common calcium oxide, magnesium oxide, zinc oxide, iron oxide, copper oxide and their hydroxides; acidic liquids include orthophosphoric acid, dihydrogen phosphate, acrylic acid, tricarboxylic acid, malic acid, tartaric acid, pyruvic acid and other acidic liquids or other acid salts soluble in water. When the alkaline oxide uses magnesium oxide or magnesium hydroxide, and the acidic component uses phosphoric acid or phosphate, it is called magnesium phosphate cement (MPC for short).

[0003] Magnesium phosphate cement has many unique properties, the most notable of which are rapid early strength development, high later strength, good volume stability, good durability and simple maintenance. Therefore, it has received great attention in recent years and has been promoted and applied.

[0004] Due to its extremely fast setting speed, the application scope of magnesium phosphate cement is limited. For a long time, it has only been used in projects such as repairs, which prevents its excellent properties from being brought into play and utilized on a larger scale.

[0005] Therefore, in the preparation and application technology of magnesium phosphate cement-based materials, effective control of setting time is the key. There have been certain studies on it at home and abroad. Among them, the more effective retarding technology is to add retarders such as boric acid. However, the use effect of the above retarders is not very ideal. There are some problems, such as: when the amount of boric acid is small, the retarding effect is not obvious, the fluidity is not good, and when the amount is large, it has an adverse effect on the early strength and late strength of magnesium phosphate cement. Summary of the invention

[0006] Therefore, the technical problem to be solved by the present invention is to overcome the defect in the prior art that boric acid is used as a retarder for magnesium phosphate cement-based materials and cannot effectively delay the setting time, improve its fluidity and at the same time improve the strength of magnesium phosphate cement and its materials, thereby providing a composite retarder for magnesium phosphate cement-based materials and its application.

[0007] The present invention provides a magnesium phosphate cement-based material composite retarder, comprising boric acid and an admixture;

[0008] The additive comprises the following raw materials: triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate;

[0009] The mass ratio of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate is (80-90):(5-12):(1-5):(2-4).

[0010] Preferably, the mass ratio of the boric acid to the additive is 1:(0.25-1).

[0011] The present invention provides an application of the above-mentioned magnesium phosphate cement-based material composite retarder in the preparation of magnesium phosphate cement-based material.

[0012] The present invention also provides a magnesium phosphate cement-based material, wherein raw materials of the magnesium phosphate cement-based material include magnesium oxide, potassium dihydrogen phosphate, water and the magnesium phosphate cement-based material composite retarder described above.

[0013] Preferably, the mass ratio of magnesium oxide to potassium dihydrogen phosphate is (1-8):1.

[0014] Preferably, the ratio of the amount of water added to the total mass of magnesium oxide, potassium dihydrogen phosphate and magnesium phosphate cement-based composite retarder is (1.5-3.0):10.

[0015] Preferably, the amount of boric acid added to the magnesium phosphate cement-based material composite retarder is 1-5% of the total mass of the magnesium phosphate cement-based material, and the amount of admixture added is 0.25-5% of the total mass of the magnesium phosphate cement-based material.

[0016] Preferably, the raw material of the magnesium phosphate cement-based material also includes sand, and the mass ratio of the total mass of the magnesium oxide, potassium dihydrogen phosphate, and magnesium phosphate cement-based material composite retarder to the sand is (0.5-2):1.

[0017] The present invention also provides a method for preparing the magnesium phosphate cement-based material described above, comprising the following steps:

[0018] Mix magnesium oxide, potassium dihydrogen phosphate and magnesium phosphate cement-based composite retarder, stir for the first time until uniform, then add water and stir for the second time. After the second stirring, pour into a mold to form.

[0019] Preferably, after the second stirring is completed, the method further comprises adding sand for a third stirring, and after the third stirring is completed, pouring the mixture into a mold for forming;

[0020] The first stirring speed is 40-80r / min, and the stirring time is 30-60s;

[0021] The second stirring speed is 40-80r / min, and the stirring time is 30-60s;

[0022] The third stirring speed is 100-140r / min, and the stirring time is 30-80s.

[0023] The technical solution of the present invention has the following advantages:

[0024] (1) The composite retarder for magnesium phosphate cement-based materials provided by the present invention comprises boric acid and an admixture; the admixture comprises the following raw materials: triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate; the mass ratio of the triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate is (80-90): (5-12): (1-5): (2-4). The present invention overcomes the defects of boric acid as a retarder for magnesium phosphate cement-based materials, that is, the retarding effect is not obvious and the strength of cement is affected, by adding an admixture. The present invention cooperates with boric acid, triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate to effectively prolong the setting time of magnesium phosphate cement-based materials, increase their fluidity, and at the same time improve the strength of magnesium phosphate cement and its materials to a certain extent.

[0025] (2) The magnesium phosphate cement-based material provided by the present invention can adjust the setting time by adjusting the amount of the composite retarder of the magnesium phosphate cement-based material, and achieve a certain early strength, especially hourly strength, while meeting the construction requirements (such as setting time and fluidity) to meet the needs of rapid repair projects. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 Hydration thermal analysis diagram of Example 1 of the present invention and Comparative Example 1. DETAILED DESCRIPTION

[0028] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0029] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0030] Example 1

[0031] The present embodiment provides a magnesium phosphate cement-based material composite retarder, which consists of boric acid and an admixture, the mass ratio of boric acid to the admixture is 1:0.25, the admixture consists of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate, and the mass ratio of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate is 90:5:1:2.

[0032] Example 2

[0033] The present embodiment provides a magnesium phosphate cement-based material composite retarder, which consists of boric acid and an admixture, the mass ratio of boric acid to the admixture is 1:0.5, the admixture consists of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate, and the mass ratio of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate is 90:5:1:2.

[0034] Example 3

[0035] The present embodiment provides a magnesium phosphate cement-based material composite retarder, which consists of boric acid and an admixture, the mass ratio of boric acid to the admixture is 1:0.75, the admixture consists of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate, and the mass ratio of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate is 90:5:1:2.

[0036] Example 4

[0037] The present embodiment provides a magnesium phosphate cement-based material composite retarder, which consists of boric acid and an admixture, the mass ratio of boric acid to the admixture is 1:1, the admixture consists of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate, and the mass ratio of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate is 90:5:1:2.

[0038] Example 5

[0039] The present embodiment provides a magnesium phosphate cement-based material composite retarder, which consists of boric acid and an admixture, the mass ratio of boric acid to the admixture is 1:0.25, the admixture consists of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate, and the mass ratio of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate is 85:8:3:4.

[0040] Example 6

[0041] The present embodiment provides a magnesium phosphate cement-based material composite retarder, which consists of boric acid and an admixture, the mass ratio of boric acid to the admixture is 1:0.5, the admixture consists of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate, and the mass ratio of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate is 85:8:3:4.

[0042] Example 7

[0043] The present embodiment provides a magnesium phosphate cement-based material composite retarder, which consists of boric acid and an admixture, the mass ratio of boric acid to the admixture is 1:0.75, the admixture consists of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate, and the mass ratio of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate is 85:8:3:4.

[0044] Example 8

[0045] The present embodiment provides a magnesium phosphate cement-based material composite retarder, which consists of boric acid and an admixture, the mass ratio of boric acid to the admixture is 1:1, the admixture consists of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate, and the mass ratio of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate is 85:8:3:4.

[0046] Example 9

[0047] The present embodiment provides a magnesium phosphate cement-based material composite retarder, which consists of boric acid and an admixture, the mass ratio of boric acid to the admixture is 1:0.25, the admixture consists of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate, and the mass ratio of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate is 80:12:5:3.

[0048] Example 10

[0049] The present embodiment provides a magnesium phosphate cement-based material composite retarder, which consists of boric acid and an admixture, the mass ratio of boric acid to the admixture is 1:0.5, the admixture consists of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate, and the mass ratio of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate is 80:12:5:3.

[0050] Embodiment 11

[0051] The present embodiment provides a magnesium phosphate cement-based material composite retarder, which consists of boric acid and an admixture, the mass ratio of boric acid to the admixture is 1:0.75, the admixture consists of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate, and the mass ratio of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate is 80:12:5:3.

[0052] Example 12

[0053] The present embodiment provides a magnesium phosphate cement-based material composite retarder, which consists of boric acid and an admixture, the mass ratio of boric acid to the admixture is 1:1, the admixture consists of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate, and the mass ratio of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate is 80:12:5:3.

[0054] Comparative Example 1

[0055] This comparative example provides a magnesium phosphate cement-based material retarder, which consists only of boric acid.

[0056] Comparative Example 2

[0057] This comparative example provides a magnesium phosphate cement-based material retarder, which consists of boric acid and an admixture, the mass ratio of boric acid to the admixture is 1:0.25, the admixture consists of triethanolamine, citric acid and sodium polyphosphate, the mass ratio of triethanolamine, citric acid and sodium polyphosphate is 90:1:2.

[0058] Comparative Example 3

[0059] This comparative example provides a magnesium phosphate cement-based material retarder, which consists of boric acid and an admixture, the mass ratio of boric acid to the admixture is 1:0.25, the admixture consists of triethanolamine, aluminum nitrate and sodium polyphosphate, the mass ratio of triethanolamine, aluminum nitrate and sodium polyphosphate is 90:5:2.

[0060] Comparative Example 4

[0061] This comparative example provides a magnesium phosphate cement-based material retarder, which consists of boric acid and an admixture, the mass ratio of boric acid to the admixture is 1:0.25, the admixture consists of triethanolamine, aluminum nitrate and citric acid, the mass ratio of triethanolamine, aluminum nitrate and citric acid is 90:5:1.

[0062] Test Case

[0063] The magnesium phosphate cement-based material composite retarder of Examples 1-12 and the magnesium phosphate cement-based material retarder of Comparative Examples 1-4 were added to magnesium phosphate cement mortar, and the fluidity, setting time, and 1d, 3d, and 7d compressive strength of the obtained magnesium phosphate cement mortar were measured.

[0064] Preparation process of magnesium phosphate cement mortar: 0.9kg magnesium oxide, 0.3kg potassium dihydrogen phosphate and the retarder described in the embodiment or comparative example are poured into a mortar mixing pot, stirred at a speed of 62r / min for 30s, water is added, stirred at a speed of 62r / min for 30s, and then standard sand is added (China ISO standard sand grade is equipped with three grades, namely coarse sand is 1.0-2.0mm, medium sand is 0.50-1.0mm, and fine sand is 0.08-0.50mm. The standard sand used is 450g of coarse sand, medium sand, and fine sand, each of which is assembled into a small bag, and the net content of each bag is 1350g), stirring is continued at a speed of 125r / min for 30s, and poured into a mold for molding. The amount of boric acid added to the magnesium phosphate cement-based material composite retarder is 2% of the total mass of the magnesium phosphate cement-based material, the ratio of the amount of water added to the total mass of magnesium oxide, potassium dihydrogen phosphate and the magnesium phosphate cement-based material composite retarder is 2:10 (i.e., the water-cement ratio), and the total mass of magnesium oxide, potassium dihydrogen phosphate and the magnesium phosphate cement-based material composite retarder The mass ratio of the standard sand is 1:1 (i.e., the lime-sand ratio);

[0065] The fluidity of magnesium phosphate cement mortar is tested according to GB / T2419-2005 standard; the initial setting time of magnesium phosphate cement mortar is tested according to JGJ / T 70-2009 "Standard for Test Methods for Basic Properties of Building Mortar" standard; the 1d, 3d, and 7d compressive strength are tested according to GB / T17671-1999 standard; the test results are shown in Table 1.

[0066] Table 1

[0067]

[0068] The cement hydration heat test was carried out on the cement in the magnesium phosphate mortar prepared by the cement retarder of Example 1 and Comparative Example 1. The test results are as follows: Figure 1 As shown in the figure, it can be seen that the hydration process of magnesium phosphate cement-based materials has two exothermic peaks. Adding the composite retarder of Example 1 can reduce the exothermic peak value and delay the time when the peak value appears, which can prove that the composite retarder has a retarding effect on magnesium phosphate cement-based materials.

[0069] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A magnesium phosphate cement-based material, characterized in that: The raw materials of the magnesium phosphate cement-based material are composed of magnesium oxide, potassium dihydrogen phosphate, water and a magnesium phosphate cement-based material composite retarder; The magnesium phosphate cement-based composite retarder consists of boric acid and an admixture; The admixture is composed of the following raw materials: triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate; The mass ratio of triethanolamine, aluminum nitrate, citric acid and sodium polyphosphate is 90:5:1:2; The mass ratio of magnesium oxide to potassium dihydrogen phosphate is (3-8):1; The mass ratio of the boric acid to the additive is 1:

1.

2. The magnesium phosphate cement-based material according to claim 1, characterized in that: The ratio of the added amount of water to the total mass of magnesium oxide, potassium dihydrogen phosphate and magnesium phosphate cement-based composite retarder is (1.5-3.0):

10.

3. The magnesium phosphate cement-based material according to claim 1 or 2, characterized in that: The amount of boric acid added to the magnesium phosphate cement-based material composite retarder is 1-5% of the total mass of the magnesium phosphate cement-based material, and the amount of the admixture added is 0.25-5% of the total mass of the magnesium phosphate cement-based material.

4. The magnesium phosphate cement-based material according to claim 1 or 2, characterized in that: The raw materials of the magnesium phosphate cement-based material also include sand, and the mass ratio of the total mass of the magnesium oxide, potassium dihydrogen phosphate, and magnesium phosphate cement-based material composite retarder to the sand is (0.5-2):

1.

5. The method for preparing the magnesium phosphate cement-based material according to any one of claims 1 to 4, characterized in that: The steps include: Mix magnesium oxide, potassium dihydrogen phosphate and magnesium phosphate cement-based composite retarder, stir for the first time until uniform, then add water and stir for the second time. After the second stirring, pour into a mold to form.

6. The method for preparing the magnesium phosphate cement-based material according to claim 5, characterized in that: After the second stirring is completed, the step of adding sand for the third stirring is also included, and after the third stirring is completed, the mixture is poured into a mold for forming; The first stirring speed is 40-80r / min, and the stirring time is 30-60s; The second stirring speed is 40-80r / min, and the stirring time is 30-60s; The third stirring speed is 100-140r / min, and the stirring time is 30-80s.