Preparation method and application of high stability water-white tackifying resin

By carrying out disproportionation hydrogenation and addition reaction of rosin under normal pressure inert gas environment, combined with esterification treatment, the problems of color stability and energy consumption in the preparation of traditional water-white tackifying resin are solved, achieving high stability and low cost. Made of high-quality resin, suitable for use in hot melt adhesives to improve adhesion and peeling force.

CN115746710BActive Publication Date: 2024-10-29GUANGXI CHORIS CHEM CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211384621.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-07
Publication Date
2024-10-29
Estimated Expiration
2042-11-07

AI Technical Summary

Technical Problem

The traditional water-white tackifying resin preparation method involves secondary melting, which increases workload and energy consumption, affects product color stability, and may cause coking and atomization during the distillation process, affecting product quality.

Method used

The refined rosin is subjected to disproportionation, hydrogenation and addition reactions under an atmospheric pressure inert gas environment, and a highly stable water-white tackifying resin is generated through an esterification reaction. A palladium carbon catalyst and fumaric acid are used. The reaction temperature and time are controlled at 200°C. ~210℃ and 1.5~2.5 hours, combined with negative pressure vacuum distillation and esterification reaction to avoid oxidation reaction and improve product stability.

Benefits of technology

It improves the stability and lightness of the product, reduces the preparation cost, is suitable for high-quality light-colored or colorless hot melt adhesives, enhances the bonding force and peeling force, and avoids the need to add additional antioxidant stabilizers. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003930198360000041
    Figure BDA0003930198360000041
  • Figure BDA0003930198360000051
    Figure BDA0003930198360000051
  • Figure BDA0003930198360000061
    Figure BDA0003930198360000061
Patent Text Reader

Abstract

The invention discloses a method for preparing a high-stability water-white tackifying resin, which comprises dissolving common rosin and distilling it under negative pressure to obtain refined rosin; adding 0.05wt% to 0.2wt% of palladium-carbon catalyst accounting for the total amount of refined rosin at 190°C to 210°C to carry out normal pressure disproportionation hydrogenation reaction with the refined rosin; adding 0.5wt% to 1.5wt% of fumaric acid accounting for the total amount of refined rosin, carrying out addition reaction, reaction temperature 200°C to 210°C, reaction time 1.5 to 2.5 hours, and then obtaining resin through esterification reaction; wherein, the disproportionation hydrogenation reaction, addition reaction, and esterification reaction are continuously stirred in an inert gas environment. The product prepared by the present invention is not only light in color, but also highly stable, which is conducive to promotion in high-quality light-colored (or colorless) hot melt adhesive products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of rosin processing, and more specifically to a preparation method and application of a high-stability water-white tackifying resin. Background Art

[0002] The traditional method for preparing water-white tackifying resin is to first produce refined rosin products from ordinary rosin as raw material, then transport the refined rosin to the resin workshop, and then react the refined rosin with polyols at high temperature to produce water-white tackifying resin. Since the traditional preparation method has a secondary melting and reaction with polyols, the workload and energy consumption are increased, and the secondary melting will deepen the color of the refined rosin. In addition, during the distillation of rosin, as the rosin liquid level decreases, coking will occur at the heating position in the kettle, and the rising atomized rosin may also be evaporated, thereby affecting the color of the product.

[0003] In this regard, the prior art, such as a method for producing a water-white tackifying resin with announcement number CN106928853B, comprises a three-stage heat transfer oil heating spiral coil arranged inside a distillation pot, and the height of the three-stage heat transfer oil heating spiral coil is arranged from high to low, and a valve is provided on each stage of the coil, and a fully enclosed three-stage distillation is used to ensure that the color of the product is close to color 0.

[0004] Although strict control of the early distillation and refining of rosin can make the product color lighter, the quality of the product still requires high stability to maintain a stable color. Summary of the invention

[0005] An object of the present invention is to solve at least the above problems and to provide at least the advantages which will be described hereinafter.

[0006] The present invention not only improves the stability of the product by performing disproportionation, hydrogenation and addition reaction on the refined rosin under a normal pressure inert gas environment, but also has good compatibility with cyclohexane oil, SIS and the like when applied in hot melt adhesives, thereby improving the adhesion and peeling strength of the adhesive product, and is conducive to the promotion of high-quality light-colored (or colorless) hot melt adhesive products.

[0007] In order to achieve these purposes and other advantages according to the present invention, the present invention provides a method for preparing a high-stability water-white tackifying resin, which comprises dissolving common rosin and performing negative pressure vacuum distillation to obtain refined rosin; adding 0.05wt% to 0.2wt% of a palladium-carbon catalyst accounting for the total amount of the refined rosin at 190° C. to 210° C. to carry out a normal pressure disproportionation hydrogenation reaction with the refined rosin; adding 0.5wt% to 1.5wt% of fumaric acid accounting for the total amount of the refined rosin to carry out an addition reaction, the reaction temperature is 200° C. to 210° C., the reaction time is 1.5 to 2.5 hours, and then performing an esterification reaction to obtain a resin; wherein the disproportionation hydrogenation reaction, the addition reaction, and the esterification reaction are carried out in an inert gas environment with continuous stirring.

[0008] Preferably, the preparation process of refined rosin is: ordinary rosin is heated to 180°C to 200°C to dissolve, and then negative pressure vacuum distillation is performed, wherein the distillation temperature is 250°C to 300°C and the pressure is -0.1Mpa, and the distilled fraction is collected as the refined rosin.

[0009] Preferably, the preparation process of the esterification reaction is as follows: after the addition reaction is completed, a polyol accounting for 25wt% to 35wt% of the total amount of the refined rosin is added for esterification reaction, the temperature is slowly raised to 270°C to 290°C for 3 hours, the reaction time is 6 to 8 hours, and the acid value of the sample is sampled and tested to be below 40, and then a negative pressure vacuum operation is performed, the temperature remains unchanged, the vacuum degree is -0.09Mpa, and the vacuum is maintained for 1.5 to 2.5 hours. The acid value index is lower than 30, and the softening point index is at 100±2°C, and the esterification reaction is completed.

[0010] Preferably, the polyol is one or both of glycerol and pentaerythritol.

[0011] Preferably, the resin obtained through the esterification reaction further comprises filtering with a filter to filter out impurities and palladium-carbon catalyst foreign matter to complete the product preparation.

[0012] Preferably, negative hydrogen ion gas is mixed into the inert gas, and the average concentration of negative hydrogen ion gas is 7×10 6 Pieces / cm 3 .

[0013] The present invention also provides a method for preparing hot melt adhesive using the water-white tackifying resin prepared by the present invention. The weight percentages of the hot melt adhesive are: cyclohexane oil: 19%; SIS elastomer: 24%; water-white tackifying resin: 42.5%; paraffin: 14%; and antioxidant: 0.5%.

[0014] Preferably, the antioxidant is antioxidant 1010.

[0015] The present invention has at least the following beneficial effects:

[0016] First, the present invention, through simple refined distillation of rosin, and sufficient disproportionation hydrogenation, addition, and esterification reactions in an inert gas environment, not only makes the product light in color, close to color 0, but also has high stability, which is conducive to promotion in high-quality light-colored (or colorless) hot melt adhesive products.

[0017] Second, the disproportionation hydrogenation of the present invention is carried out under normal pressure, which is different from the conventional use of a dedicated high-pressure hydrogenation system, and can save preparation costs.

[0018] Third, the negative hydrogen ion gas is introduced into the disproportionation, hydrogenation, addition and esterification reaction processes of the present invention, which can not only avoid oxidation reaction during the reaction process, but also further promote the full reaction of disproportionation and hydrogenation, and make unsaturated organic matter become saturated organic matter, and further improve product stability. In addition, the negative hydrogen ion gas in the sealed stainless steel reactor can reduce the partially oxidized refined rosin, reduce the product color, and improve the quality.

[0019] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. DETAILED DESCRIPTION

[0020] The present invention is further described in detail below in conjunction with embodiments so that those skilled in the art can implement the invention with reference to the description.

[0021] It should be understood that terms such as “having”, “including” and “comprising” used herein do not specify the existence or addition of one or more other elements or combinations thereof.

[0022] It should be noted that the experimental methods described in the following embodiments are conventional methods unless otherwise specified, and the reagents and materials can be obtained from commercial channels unless otherwise specified.

[0023] <Example 1>

[0024] A method for preparing a high-stability water-white tackifying resin, namely, the detailed preparation steps of resin No. 1 include:

[0025] Step 1, refined distillation: ordinary rosin (Pinus massoniana) is heated to 200℃ and dissolved, and then negative pressure vacuum distillation is performed. During distillation, the temperature is slowly increased from 250℃ to 290℃, and the pressure is -0.1Mpa. The distilled fraction is collected as refined rosin, and the recovery rate is about 90%;

[0026] Step 2, disproportionation and hydrogenation: the distilled rosin is transferred to an esterification reactor (disproportionation, hydrogenation and esterification are carried out simultaneously), and a palladium carbon catalyst accounting for 0.1wt% of the total amount of refined rosin is added at about 200°C to carry out disproportionation and hydrogenation reactions under normal pressure (the reaction is carried out throughout the whole process, and the degree of reaction is related to the amount and type of the catalyst added);

[0027] Step 3, addition reaction: then add 1%wt of fumaric acid based on the total amount of refined rosin into the reactor to carry out addition reaction at a reaction temperature of 200°C for a reaction time of 2 hours;

[0028] Step 4, esterification reaction: after the addition reaction is completed, add 30wt% of the total amount of refined rosin (the polyol is selected from glycerol and pentaerythritol, and the proportion of glycerol is very small, specifically, 3wt% of the total amount of refined rosin and 27wt% of the total amount of refined rosin are added) for esterification reaction, slowly heat up for 3 hours to 290° C., react for 6 hours, take samples to detect that the acid value of the sample is below 40, and then perform negative pressure vacuuming operation, the temperature remains unchanged, the vacuum degree is -0.09Mpa, and the vacuum is maintained for about 2 hours. The acid value index is lower than 30 and the softening point index is at 100±2° C., that is, the esterification reaction is completed;

[0029] Step 5: Filter through a filter to filter out impurities, palladium-carbon catalyst and other foreign matters to complete product preparation; wherein the disproportionation hydrogenation reaction, addition reaction, and esterification reaction are continuously stirred in an inert gas environment, such as nitrogen.

[0030] <Example 2>

[0031] Detailed preparation steps of resin No. 2:

[0032] Without distillation, ordinary rosin is directly used for hydrogenation and disproportionation, and steps 2, 3, 4, and 5 are the same as above.

[0033] <Example 3>

[0034] Detailed preparation steps of resin No. 3:

[0035] Step 1 is the same as Resin No. 1; after distillation is completed, proceed to Steps 3, 4, and 5.

[0036] <Example 4>

[0037] Detailed preparation steps of resin No. 4:

[0038] Steps 1 and 2 are the same as for resin No. 1; skip step 3 and go directly to steps 4 and 5.

[0039] <Example 5>

[0040] Detailed preparation steps of resin No. 5:

[0041] Steps 1, 2, 3, 4, and 5 are the same as those of Resin No. 1, and the disproportionation hydrogenation, addition, and esterification reactions are carried out in a sealed stainless steel reactor. The difference is that negative hydrogen ion gas is mixed into the inert gas, that is, negative hydrogen ion gas is mixed into the nitrogen, and the average concentration of the negative hydrogen ion gas is 7×10 6 Pieces / cm 3 .

[0042] The resin indicators prepared by the comparative experiment are as follows:

[0043] Table 1:

[0044]

[0045]

[0046] It is obvious from the resin index data tested in Table 1 that the present invention not only makes the product lighter in color and lower in acid value but also has high stability through simple refined distillation of rosin and sufficient disproportionation hydrogenation, addition, and esterification reaction in an inert gas environment mixed with negative hydrogen ions, which is conducive to the promotion and application of high-quality light-colored (or colorless) hot melt adhesive products.

[0047] Resin antioxidant performance test:

[0048] (Put the resin in a test tube with a diameter of 1 cm, place it in an oven at 180°C, and observe the degree of color change)

[0049] Table 2:

[0050] Initial color number Place in oven at 180°C for 24 hours Resin No. 1 Color 0.5 Color 1.0 Resin No. 2 Color 1.8 Color 2.3 Resin No. 3 Color 0.9 Color 2.5 No. 4 resin Color 0.4 Color 1.0 Resin No. 5 Color 0.1 Color 0.2

[0051] The antioxidant performance test in Table 2 further illustrates that the present invention not only makes the product lighter in color, but also has high stability and small color change range through simple refined distillation of rosin and sufficient disproportionation hydrogenation, addition, and esterification reactions in an inert gas environment mixed with negative hydrogen ions. The product can maintain a stable color without adding additional antioxidant stabilizers, which is conducive to the promotion and application of high-quality light-colored (or colorless) hot melt adhesive products.

[0052] The present invention also provides the high stability water-white tackifying resin of the present invention used in the preparation of hot melt adhesive as follows:

[0053] The hot melt adhesive formula is as follows: naphthenic oil: 19%; SIS elastomer: 24%; water-white tackifying resin: 42.5%; paraffin: 14%; antioxidant (antioxidant 1010): 0.5%.

[0054] Preparation steps: Add the substances in the above formula into the reactor, heat to 180°C, stir thoroughly and evenly until the material becomes transparent, pour out and cool, and the hot melt adhesive is prepared. However, to test its initial adhesion, lasting adhesion and peeling strength, it is necessary to coat it and make the corresponding tape for measurement. The measurement results are shown in Table 3.

[0055] 1. Ring initial adhesion test:

[0056] ⑴. Testing equipment

[0057] Device Name model High and low temperature material tensile testing machine LK-103B

[0058] ⑵Environmental conditions

[0059] Temperature: 25.2℃ Humidity: 45%

[0060] Test conditions:

[0061] Pasting area: 25×25mm, test speed: 300mm / min

[0062] 2. 70℃500g adhesion test

[0063] ⑴Testing equipment

[0064] Device Name model Constant temperature tape adhesion tester LK-601B

[0065] ⑵Environmental conditions

[0066] Temperature: 25.8℃ Humidity: 52%

[0067] Test conditions:

[0068] Load: 500g Pasting area: 25×25mm Test temperature: 70℃

[0069] Note: After pasting, use a 2Kg roller to press back and forth 3 times. Test after leaving it for 1 hour and record the final fall-off time.

[0070] 3. 180° peel strength test

[0071] Test method: GB / T 2792-2014 "Test method for peel strength of adhesive tape".

[0072] Table 3:

[0073]

[0074]

[0075] From the test resin application data in Table 3, it is obvious that the high stability water-white tackifying resin prepared by the present invention is applied in hot melt adhesive, has good compatibility with naphthenic oil, SIS, etc., improves the adhesion and peeling force of the adhesive product, and is conducive to its application in hot melt adhesive products. Moreover, during the disproportionation, hydrogenation, addition and esterification reactions, the introduction of negative hydrogen ion gas can further improve the adhesion and peeling force of the hot melt adhesive product, and has great prospects for application in high-quality light-colored (or colorless) hot melt adhesive products.

[0076] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the examples shown and described herein.

Claims

1. A method for preparing a water-white tackifying resin, characterized in that: The method comprises dissolving common rosin and performing negative pressure vacuum distillation to obtain refined rosin; adding 0.05wt%~0.2wt% of palladium carbon catalyst accounting for the total amount of refined rosin at 190℃~210℃ to carry out normal pressure disproportionation hydrogenation reaction with the refined rosin; adding 0.5wt%~1.5wt% of fumaric acid accounting for the total amount of refined rosin to carry out addition reaction, the reaction temperature is 200℃~210℃, the reaction time is 1.5~2.5 hours, and then carrying out esterification reaction to obtain resin; wherein the disproportionation hydrogenation reaction, the addition reaction, and the esterification reaction are continuously stirred in an inert gas environment, and negative hydrogen ion gas is mixed into the inert gas, and the average concentration of the negative hydrogen ion gas is 7×10 6 Pieces / cm 3 .

2. The method for preparing a water-white tackifying resin according to claim 1, wherein The preparation process of the refined rosin is as follows: ordinary rosin is heated to 180°C-200°C to dissolve, and then negative pressure vacuum distillation is performed at a temperature of 250°C-300°C, and the distilled fraction is collected to obtain the refined rosin.

3. The method for preparing a water-white tackifying resin according to claim 2, wherein: The preparation process of the esterification reaction is as follows: after the addition reaction is completed, 25wt%~35wt% of the polyol accounting for the total amount of the refined rosin is added to carry out the esterification reaction, the temperature is raised to 270°C~290°C for 2-3 hours, the reaction time is 6-8 hours, and the acid value of the sample is detected to be below 40, and then a negative pressure vacuum operation is carried out, the temperature remains unchanged, and the vacuum is maintained for 1.5-2.5 hours. When the acid value index is lower than 30 and the softening point index is at 100±2°C, the esterification reaction is completed.

4. The method for preparing a water-white tackifying resin according to claim 3, wherein: The polyol is one or both of glycerol and pentaerythritol.

5. The method for preparing a water-white tackifying resin according to claim 1, wherein The resin obtained through the esterification reaction also includes filtering with a filter to filter out impurities and palladium-carbon catalyst foreign matter to complete the product preparation.

6. Hot melt adhesive, characterized in that: The water-white tackifying resin prepared as claimed in any one of claims 1 to 5 is used to prepare the hot melt adhesive in the following weight percentages: 19% cyclohexane oil; 24% SIS elastomer; 42.5% water-white tackifying resin; 14% paraffin wax; and 0.5% antioxidant.

7. The hot melt adhesive according to claim 6, characterized in that: The antioxidant is antioxidant 1010.

Citation Information

Patent Citations

  • A method for producing a water-white tackifying resin

    CN106928853B

  • Preparation method of hydrogenated rosin imitated resin type novel hot melt adhesive

    CN106590472A

  • High-persistent-adhesion hot melt adhesive for hook and preparation method of high-persistent-adhesion hot melt adhesive

    CN114456749A