Negative electrode for nonaqueous electrolyte secondary battery, nonaqueous electrolyte secondary battery, and method for producing negative electrode for nonaqueous electrolyte secondary battery

By using silicon compound particles covered with silyl groups in the negative electrode active material of lithium-ion secondary batteries, the problem of poor circulation characteristics and primary efficiency of silicon materials in lithium-ion secondary batteries is solved, and high capacity and good quality are achieved The cycle maintenance rate is suitable for industrial production.

CN115763806BActive Publication Date: 2024-11-08SHIN ETSU CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211456461.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2017-06-02
Filing Date
2018-05-18
Publication Date
2024-11-08
Estimated Expiration
2038-05-18

AI Technical Summary

Technical Problem

When using silicon material as the negative electrode material, existing lithium-ion secondary batteries have problems of poor circulation characteristics and primary efficiency, and the modified silicon oxide has low water resistance, resulting in insufficient slurry stability and difficult to produce in industrial production. Applied in.

Method used

Using silicon compound particles (SiOx: 0.5≤x≤1.6) as the negative electrode active substance, a compound layer with silyl group is formed on the surface of silicon compound particles or the surface of carbon material, to inhibit the aggregation of active substances and improve conductivity, and to form a high capacity , Non-aqueous electrolyte secondary battery with good circulation characteristics.

Benefits of technology

It has achieved the improvement of the stability and battery capacity of the secondary battery paste, enhanced the cycle maintenance rate and primary charging and discharge characteristics, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115763806B_ABST
    Figure CN115763806B_ABST
Patent Text Reader

Abstract

The present invention is a negative electrode active material for a non-aqueous electrolyte secondary battery, which comprises negative electrode active material particles. The negative electrode active material for a non-aqueous electrolyte secondary battery is characterized in that: the negative electrode active material particles contain a silicon compound (SiO x :0.5≤x≤1.6), the silicon compound particles contain a Li compound, at least a portion of the silicon compound particles is covered by a carbon material, and the surface of the silicon compound particles or the surface of the carbon material or at least a portion of the two surfaces is covered by a layer containing a compound having a silyl group. Thus, a negative electrode active material for a non-aqueous electrolyte secondary battery is provided, which has high stability to an aqueous slurry and a high capacity, and has good cycle characteristics and initial efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention is a divisional application of the Chinese patent application with application number 201880036598.6, application date May 18, 2018, and invention name “Negative electrode active material for non-aqueous electrolyte secondary battery, preparation method thereof, and non-aqueous electrolyte secondary battery containing the same”. This application claims priority based on patent application No. 2017-109785 filed in Japan on June 2, 2017. Technical Field

[0002] The present invention relates to a negative electrode active material for a non-aqueous electrolyte secondary battery, a non-aqueous electrolyte secondary battery, and a method for preparing the negative electrode material for the non-aqueous electrolyte secondary battery. Background Art

[0003] In recent years, small electronic devices represented by mobile terminals have become widely popular, and there is a strong demand for further miniaturization, lightness and longevity. In response to such market demand, the development of a secondary battery that is particularly small and light and can obtain high energy density has been promoted. The application of this secondary battery is not limited to small electronic devices, and its application in large electronic devices represented by automobiles and power storage systems represented by houses is also under study.

[0004] Among them, lithium-ion secondary batteries are expected to be easy to reduce in size and increase in capacity, and can achieve higher energy density than lead batteries and nickel-cadmium batteries.

[0005] The lithium ion secondary battery comprises a positive electrode, a negative electrode, a separator and an electrolyte, and the negative electrode contains a negative electrode active material involved in charge and discharge reactions.

[0006] As the negative electrode active material, carbon materials are widely used, but according to the recent market demand, the battery capacity is sought to be further improved. In order to increase the battery capacity, the use of silicon as the negative electrode active material is being studied. The reason is that the theoretical capacity of silicon (4199mAh / g) is more than 10 times that of graphite (372mAh / g), so it can be expected to greatly increase the battery capacity. For the development of silicon materials as negative electrode active material materials, not only silicon single substance is studied, but also compounds represented by alloys and oxides are studied. In addition, regarding the shape of the active material, for carbon materials, there are studies ranging from standard coating types to integrated types directly deposited on the collector.

[0007] However, if silicon is used as the main material for the negative electrode active material, the negative electrode active material will expand and shrink during charge and discharge, and therefore, it will become easy to break, mainly near the surface of the negative electrode active material. In addition, ionic substances will be generated inside the active material, and the negative electrode active material will become a substance that is easy to break. If the surface of the negative electrode active material breaks, a new surface will be generated, and the reaction area of ​​the active material will increase. At this time, since the decomposition reaction of the electrolyte occurs on the new surface, and at the same time a film of the decomposition product of the electrolyte is formed on the new surface, the electrolyte will be consumed. Therefore, the cycle characteristics of the battery become easy to reduce.

[0008] Hitherto, various studies have been conducted on negative electrode materials and electrode structures for lithium-ion secondary batteries using silicon materials as main materials in order to improve the initial efficiency and cycle characteristics of the battery.

[0009] Specifically, in order to obtain good cycle characteristics and high safety, a vapor phase method is used to simultaneously deposit silicon and amorphous silicon dioxide (for example, refer to patent document 1). In addition, in order to obtain high battery capacity and safety, a carbon material (conductive material) is provided on the surface layer of the silicon oxide particles (for example, refer to patent document 2). Furthermore, in order to improve the cycle characteristics and obtain high input-output characteristics, an active material containing silicon and oxygen is prepared, and an active material layer having a higher oxygen ratio near the collector is formed (for example, refer to patent document 3). In addition, in order to improve the cycle characteristics, oxygen is contained in the silicon active material, and is formed in a manner such that the average oxygen content is less than 40at% and the oxygen content near the collector is higher (for example, refer to patent document).

[0010] In addition, in order to improve the initial charge and discharge efficiency, a Si phase, SiO2, M y O metal oxide nanocomposite (for example, refer to Patent Document 5). In addition, in order to improve the cycle characteristics, SiO x (0.8≤x≤1.5, particle size range = 1μm to 50μm) is mixed with a carbon material and calcined at a high temperature (for example, refer to Patent Document 6). In addition, in order to improve the cycle characteristics, the molar ratio of oxygen to silicon in the negative electrode active material is set to 0.1 to 1.2, and the active material is controlled in a range where the difference between the maximum and minimum values ​​of the molar ratio near the interface between the active material and the collector is less than 0.4 (for example, refer to Patent Document 7). In addition, in order to improve the load characteristics of the battery, a metal oxide containing lithium is used (for example, refer to Patent Document 8).

[0011] In addition, as a method for suppressing particle agglomeration, it is reported that the particle surface is treated with silane compounds (for example, see Patent Document 9). In addition, in order to suppress the amount of water entering the battery, the surface of the inorganic particles is hydrophobized (for example, see Patent Document 10). In order to improve the cycle characteristics, a hydrophobic layer such as a silane compound is formed on the surface of the silicon material (for example, see Patent Document 11).

[0012] Prior art literature

[0013] Patent Literature

[0014] Patent Document 1: Japanese Patent Application Publication No. 2001-185127

[0015] Patent Document 2: Japanese Patent Application Publication No. 2002-042806

[0016] Patent Document 3: Japanese Patent Application Publication No. 2006-164954

[0017] Patent Document 4: Japanese Patent Application Publication No. 2006-114454

[0018] Patent Document 5: Japanese Patent Application Publication No. 2009-070825

[0019] Patent Document 6: Japanese Patent Application Publication No. 2008-282819

[0020] Patent Document 7: Japanese Patent Application Publication No. 2008-251369

[0021] Patent Document 8: Japanese Patent Application Publication No. 2008-177346

[0022] Patent Document 9: Japanese Patent Application Publication No. 2000-044226

[0023] Patent Document 10: Japanese Patent No. 5160544

[0024] Patent Document 11: Japanese Patent Application Publication No. 2007-234255 Summary of the invention

[0025] Technical Problems to be Solved by the Invention

[0026] As mentioned above, in recent years, small electronic devices represented by mobile terminals have been increasingly becoming more high-performance and multifunctional, requiring the battery capacity of lithium-ion secondary batteries, which are their main power sources, to increase. As a method of solving this problem, it is desirable to develop a lithium-ion secondary battery comprising a negative electrode using a silicon material as the main material.

[0027] In addition, it is expected that the battery characteristics of lithium ion secondary batteries using silicon materials are similar to those of lithium ion secondary batteries using carbon materials. Therefore, silicon oxide modified by the absorption and partial detachment of Li is used as a negative electrode active material, thereby improving the cycle maintenance rate and initial efficiency of the battery. However, the modified silicon oxide is modified by using Li, so the water resistance is low. Therefore, the stabilization of the slurry containing the above-mentioned modified silicon oxide produced when manufacturing the negative electrode will become insufficient, and the slurry will sometimes produce gas as time changes. When applying carbon-based active materials, there is a situation where the commonly used devices in the past cannot be used, or there is a problem that these devices are not easy to use. In addition, there is a problem that the silicon compound particles modified by using Li have strong agglomeration, so the slurry cannot be applied. In this way, in the case of using silicon oxide modified by using Li to improve the initial efficiency and cycle maintenance rate, the stability of the aqueous slurry becomes insufficient, so a non-aqueous electrolyte secondary battery negative electrode active material with advantages in the industrial production of secondary batteries has not yet been proposed.

[0028] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a negative electrode active material for a non-aqueous electrolyte secondary battery which has high stability in an aqueous slurry, high capacity, and excellent cycle characteristics and initial efficiency.

[0029] Technical means to solve technical problems

[0030] In order to achieve the above object, the present invention provides a negative electrode active material for a non-aqueous electrolyte secondary battery, which comprises negative electrode active material particles. The negative electrode active material for a non-aqueous electrolyte secondary battery is characterized in that:

[0031] The negative electrode active material particles contain a silicon compound (SiO x : 0.5≤x≤1.6) silicon compound particles,

[0032] The silicon compound particles contain a Li compound,

[0033] At least a portion of the silicon compound particles is covered with a carbon material,

[0034] The surface of the silicon compound particle or the surface of the carbon material or at least a part of both surfaces is covered with a layer containing a compound having a silyl group.

[0035] For the negative electrode active material of the present invention, since the negative electrode active material particles containing silicon compound particles have a compound with a silyl group on their outermost surface, when making an electrode, it is possible to inhibit the aggregation of active materials with each other and improve the water resistance to aqueous slurry. In addition, in the present invention, since at least a portion of the surface of the silicon compound particles is covered by a carbon material (hereinafter, also referred to as a carbon coating), the conductivity is excellent. Therefore, if the negative electrode active material of the present invention is used, a non-aqueous electrolyte secondary battery can be advantageously manufactured in industrial production, which makes use of the original properties of silicon oxide modified using Li, and has a high battery capacity and a good cycle retention rate. In addition, below, the negative electrode active material particles containing silicon compound particles are also referred to as silicon-based active material particles. In addition, the negative electrode active material containing the silicon-based active material particles is also referred to as a silicon-based active material.

[0036] Furthermore, it is preferred that the silyl group be a silyl group having an organic group having 1 to 5 carbon atoms.

[0037] Such a silyl group can impart appropriate hydrophobicity to the negative electrode active material particles.

[0038] Furthermore, it is preferred that at least a portion of the silicon compound particles contain at least one selected from the group consisting of Li4SiO4, Li2SiO3, and Li2Si2O5.

[0039] Lithium silicates such as Li4SiO4, Li2SiO3, and Li2Si2O5 are relatively stable as lithium compounds, and therefore can achieve better battery characteristics.

[0040] Furthermore, it is preferred that the coverage amount of the carbon material is 0.5 mass % or more and 15 mass % or less based on the total of the silicon compound particles and the carbon material.

[0041] When the coverage amount of the carbon material is within this range, negative electrode active material particles having high capacity and excellent electrical conductivity can be obtained.

[0042] Furthermore, the negative electrode active material particles preferably have a volume resistivity of 0.01 Ω·cm or more and less than 100 Ω·cm when 38.2 MPa is applied as measured by a four-probe method in accordance with JIS K7194.

[0043] When the volume resistivity is 0.01 Ω·cm or more and less than 100 Ω·cm, sufficient conductivity can be ensured, and thus better battery characteristics can be obtained.

[0044] Furthermore, it is preferred that the half-value width (2θ) of the diffraction peak caused by the Si (111) crystal plane obtained by X-ray diffraction of the silicon compound particles is 1.2° or more, and the crystallite size corresponding to the crystal plane is 7.5 nm or less.

[0045] Silicon compound particles having such a crystallite size have low crystallinity and a small amount of Si crystals, and thus can improve battery characteristics.

[0046] Furthermore, it is preferred that the silicon compound particles have a median particle size of 0.5 μm or more and 20 μm or less.

[0047] If the median particle size is 0.5 μm or more, the area where side reactions occur on the surface of the silicon compound particles is small, so no extra Li is consumed, and the high cycle retention rate of the battery can be maintained. In addition, if the median particle size is 20 μm or less, the expansion during Li absorption is small, and it is not easy to break and crack. Furthermore, since the silicon compound particles expand little, for example, the negative electrode active material layer in which a carbon-based active material is mixed with a commonly used silicon-based active material is not easily damaged.

[0048] Furthermore, the present invention provides a non-aqueous electrolyte secondary battery, characterized by comprising the negative electrode active material for a non-aqueous electrolyte secondary battery of the present invention.

[0049] Such a secondary battery has high cycle retention rate and primary efficiency and can be manufactured with industrial advantages.

[0050] Furthermore, the present invention provides a method for preparing a negative electrode material for a non-aqueous electrolyte secondary battery, wherein the negative electrode material for a non-aqueous electrolyte secondary battery comprises negative electrode active material particles containing silicon compound particles, and the method for preparing a negative electrode material for a non-aqueous electrolyte secondary battery is characterized in that it comprises the following steps:

[0051] Making silicon compounds (SiO x :0.5≤x≤1.6) of silicon compound particles;

[0052] A step of covering at least a portion of the silicon compound particles with a carbon material;

[0053] A step of modifying the silicon compound particles by absorbing lithium into the silicon compound particles; and

[0054] A step of forming a layer containing a compound having a silyl group on the surface of the modified silicon compound particles or the surface of the carbon material or on at least a part of both surfaces;

[0055] A negative electrode material for a non-aqueous electrolyte secondary battery is prepared by using the silicon compound particles on which the layer containing the compound having a silyl group is formed as negative electrode active material particles.

[0056] If this method is used to prepare a negative electrode material for a non-aqueous electrolyte secondary battery, a negative electrode material for a non-aqueous electrolyte secondary battery can be obtained that utilizes the original properties of silicon oxide modified by using Li and has a high battery capacity and a good cycle retention rate. Furthermore, since the negative electrode material prepared in this way contains silicon-based active material particles having a layer containing a compound having a silyl group as described above, the slurry prepared when manufacturing the negative electrode becomes stable. That is, a negative electrode material that can be advantageously produced for secondary batteries in an industrial manner can be obtained.

[0057] Effects of the Invention

[0058] The negative electrode active material of the present invention can improve the stability of the slurry made when manufacturing a secondary battery. If this slurry is used, an industrially usable coating can be formed, so the battery capacity, cycle characteristics and initial charge and discharge characteristics can be substantially improved. In addition, the secondary battery of the present invention comprising the negative electrode active material can be produced industrially to become a secondary battery with good battery capacity, cycle characteristics and initial charge and discharge characteristics. In addition, electronic equipment, power tools, electric vehicles and power storage systems using the secondary battery of the present invention can also obtain the same effect.

[0059] In addition, the method for preparing the negative electrode material of the present invention can prepare a negative electrode material that can improve the stability of the slurry prepared when manufacturing a secondary battery, and can improve the battery capacity, cycle characteristics, and initial charge and discharge characteristics. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] Figure 1 This is a schematic diagram showing the structure of the silicon-based active material particles contained in the negative electrode active material of the present invention, in the vicinity of the layer containing the compound having a silyl group.

[0061] Figure 2 It is a cross-sectional view showing the structure of a negative electrode including the negative electrode active material of the present invention.

[0062] Figure 3 This is a schematic diagram showing an example of an in-body reforming device that can be used when producing the negative electrode active material of the present invention.

[0063] Figure 4 It is an exploded view showing a configuration example (laminated film type) of a lithium ion secondary battery including the negative electrode active material of the present invention. DETAILED DESCRIPTION

[0064] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.

[0065] As described above, as a method for increasing the battery capacity of a lithium ion secondary battery, the use of the following negative electrode as the negative electrode of the lithium ion secondary battery has been studied, and the negative electrode uses a silicon-based active material as the main material. Although it is expected that the cycle characteristics and initial efficiency of the lithium ion secondary battery using the silicon-based active material as the main material are similar to the cycle characteristics and initial efficiency of the lithium ion secondary battery using the carbon material, the silicon-based active material modified by using Li in order to obtain the cycle characteristics and initial efficiency similar to those of the lithium ion secondary battery using the carbon material is not easy to make a stable slurry, and it is difficult to manufacture a negative electrode of good quality.

[0066] Therefore, the inventors of the present application have repeatedly and earnestly studied to obtain a negative electrode active material for a non-aqueous electrolyte secondary battery that can easily produce a high battery capacity and has good cycle characteristics and initial efficiency, and have completed the present invention.

[0067] The negative electrode active material of the present invention comprises negative electrode active material particles. The negative electrode active material particles contain a silicon compound (SiO x :0.5≤x≤1.6). The silicon compound particles contain a Li compound. In addition, at least a portion of the silicon compound particles is covered with a carbon material. Furthermore, the surface of the silicon compound particles or the surface of the carbon material or at least a portion of both surfaces is covered with a layer containing a compound having a silyl group.

[0068] Here, Figure 1 FIG. 4 shows an outline of the surface layer and the vicinity of the silicon compound particle 1. Figure 1 As shown in FIG. 1 , a carbon coating 2 is formed on the surface of the silicon compound particle 1. Figure 1 In the case of the carbon coating, a carbon coating is formed on a portion of the surface of the silicon compound particle, but the carbon coating may be formed on the entire surface of the silicon compound particle. In addition, a layer (silyl region) 3 containing a compound having a silyl group is formed on the surface of the silicon compound particle 1 and the surface of the carbon coating 2. Figure 1 In the above, an example is given in which the silyl group in the layer 3 containing the compound having a silyl group is a trimethylsilyl group, but the present invention is not particularly limited thereto.

[0069] In this negative electrode active material, since the silicon-based active material particles have silyl groups such as alkylsilyl groups on their outermost surface, the aggregation of the silicon-based active material particles is suppressed, and further, the water resistance to the aqueous slurry becomes higher. In the past, silicon oxide modified by the absorption and detachment of Li was easily agglomerated in the aqueous slurry, and further produced gas over time, so it was not suitable for mass production. However, in the present invention, by making the silicon-based active material particles have the above-mentioned layer containing the compound with silyl groups, the aggregation in the slurry is suppressed, and the slurry is not easy to produce gas with time, a stable coating can be obtained, and the adhesion can be fully ensured. In addition, since at least a part of the surface of the silicon compound particles of the present invention is covered by a carbon coating, the conductivity is excellent. Therefore, if the negative electrode active material of the present invention is used, a non-aqueous electrolyte secondary battery can be advantageously manufactured in industrial production, which makes use of the original characteristics of silicon oxide modified using Li, and has a high battery capacity and a good cycle retention rate. The coverage amount of the layer containing the compound having a silyl group is not particularly limited, and can be set to 10% by mass or less relative to the negative electrode active material particles, for example. In addition, the lower limit of the coverage amount is as long as a layer containing the compound having a silyl group can be formed on the surface of the negative electrode active material particles, and can be set to 0.01% by mass or more relative to the negative electrode active material particles.

[0070] [Constitution of negative electrode]

[0071] Next, the structure of the negative electrode of the secondary battery containing the negative electrode active material of the present invention will be described.

[0072] Figure 2 1 is a cross-sectional view of a negative electrode containing the negative electrode active material of the present invention. Figure 2 As shown, the negative electrode 10 has a structure having a negative electrode active material layer 12 on a negative electrode collector 11. The negative electrode active material layer 12 may be provided on both sides or only on one side of the negative electrode collector 11. Furthermore, in the negative electrode of the nonaqueous electrolyte secondary battery of the present invention, the negative electrode collector 11 may not be present.

[0073] [Negative electrode current collector]

[0074] The negative electrode current collector 11 is an excellent conductive material and is composed of a material having excellent mechanical strength. Examples of conductive materials that can be used for the negative electrode current collector 11 include copper (Cu) and nickel (Ni). The conductive material is preferably a material that does not form an intermetallic compound with lithium (Li).

[0075] It is preferred that the negative electrode current collector 11 contains carbon (C) and sulfur (S) in addition to the main elements. The reason is that the physical strength of the negative electrode current collector can be improved. The reason is also that, especially in the case of an active material layer that expands during charging, if the current collector contains the above elements, it has the effect of suppressing deformation of the electrode containing the current collector. Although the content of the above-mentioned elements is not particularly limited, it is preferably less than 100 ppm. The reason is that a higher effect of suppressing deformation can be obtained.

[0076] The surface of the negative electrode current collector 11 may be roughened or not. The roughened negative electrode current collector is, for example, a metal foil that has been electrolytically treated, embossed, or chemically etched. The unroughened negative electrode current collector is, for example, a rolled metal foil.

[0077] [Negative Electrode Active Material Layer]

[0078] In addition to silicon-based active material particles, the negative electrode active material layer 12 may also include a variety of negative electrode active materials such as carbon-based active materials. Further, considering the battery design, other materials such as thickeners (also called "adhesives" or "binders") and conductive additives may also be included. In addition, the shape of the negative electrode active material may be granular.

[0079] As described above, the negative electrode active material of the present invention comprises silicon compound particles, and the silicon compound particles are silicon compounds (SiO x : 0.5≤x≤1.6), and preferably x is close to 1. This is because high cycle characteristics can be obtained. In addition, the composition of the silicon oxide material in the present invention does not necessarily mean that the purity is 100%, and it may also contain trace amounts of impurity elements or Li.

[0080] In addition, in the present invention, the lower the crystallinity of the silicon compound, the better. Specifically, it is expected that the half-value width (2θ) of the diffraction peak caused by the Si (111) crystal plane obtained by X-ray diffraction of the silicon compound particles is 1.2° or more, and the crystallite size corresponding to the crystal plane is 7.5nm or less. The crystallite size can be calculated from the half-value width of the diffraction peak caused by the Si (111) crystal plane obtained by X-ray diffraction. In this way, especially due to the low crystallinity and the small amount of Si crystals present, not only can the battery characteristics be improved, but also stable lithium compounds can be generated.

[0081] In addition, the median particle size of the silicon compound particles is not particularly limited, and is preferably greater than 0.5 μm and less than 20 μm. The reason is that if it is within this range, the storage and release of lithium ions during charging and discharging becomes easy, and at the same time, the silicon-based active material particles become less likely to break. If this median particle size is greater than 0.5 μm, the surface area will not be too large, so side reactions are less likely to occur during charging and discharging, and the irreversible capacity of the battery can be reduced. On the other hand, if the median particle size is less than 20 μm, the silicon-based active material particles are less likely to break and less likely to produce new surfaces, so it is preferred.

[0082] Furthermore, in the present invention, it is preferred that the silicon-based active material contains at least one selected from Li4SiO4, Li2SiO3, and Li2Si2O5 as a lithium compound contained in at least a portion of the silicon compound particles. Compared with other lithium compounds, lithium silicates such as Li4SiO4, Li2SiO3, and Li2Si2O5 are relatively stable, so the silicon-based active material containing these lithium compounds can obtain more stable battery characteristics. These lithium compounds can be obtained by modifying the silicon compound particles by selectively replacing a part of the SiO2 component generated inside the silicon compound particles with lithium compounds.

[0083] The lithium compound inside the silicon compound particles can be quantified by NMR (nuclear magnetic resonance) and XPS (X-ray photoelectron spectroscopy). XPS and NMR measurements can be performed, for example, under the following conditions.

[0084] XPS

[0085] Device: X-ray photoelectron spectrometer

[0086] X-ray source: monochromatized Al Kα rays

[0087] X-ray focal spot diameter: 100μm

[0088] Ar ion gun sputtering conditions: 0.5kV 2mm×2mm

[0089] 29 Si MAS NMR (Magic Angle Spinning Nuclear Magnetic Resonance)

[0090] · Apparatus: 700NMR spectrometer manufactured by Bruker

[0091] Probe: 4mm HR-MAS rotor 50μL

[0092] Sample rotation speed: 10kHz

[0093] ·Measurement environment temperature: 25℃

[0094] In addition, in the present invention, when modifying the silicon compound particles, electrochemical methods, or modification based on redox reactions, and methods such as thermal doping as physical methods can be used. In particular, when the silicon compound particles are modified using electrochemical methods and redox-based modifications, the battery characteristics of the negative electrode active material are improved. In addition, the modification can be performed not only by absorbing lithium into the silicon compound particles, but also by stabilizing the lithium compound based on heat treatment and separating lithium from the silicon compound particles. As a result, the water resistance of the negative electrode active material and the stability of the slurry can be further improved.

[0095] In the negative electrode active material of the present invention, the silicon compound particles preferably have 29 The peak derived from the SiO2 region is presented at -95 to -150 ppm as the chemical shift value obtained by Si-MAS-NMR spectrum. In this way, the SiO2 region in the silicon compound particles is not completely replaced by lithium compounds through modification, but a certain degree of SiO2 region remains, which further improves the stability of the slurry.

[0096] Furthermore, as described above, the silicon-based active material particles have a layer containing a compound having a silyl group on the surface of the silicon compound particles or the surface of the carbon coating.

[0097] As a silyl group, a silyl group having an organic group such as an alkyl group can be listed. At this time, a silyl group having an organic group having 1 to 5 carbon atoms is preferred. A silyl group having an alkyl group having 1 to 5 carbon atoms is further preferred. At this time, the alkyl group is preferably a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a tert-butyl group, and an isobutyl group. When the alkyl chain has a carbon number of 5 or less, the hydrophobicity will not become too strong, and the dispersibility of the aqueous slurry will not deteriorate easily. As a silyl group having such an alkyl group, trialkylsilyl groups such as a trimethylsilyl group and a triethylsilyl group can be listed. At this time, the three alkyl groups may be the same as described above, or they may be different. In addition, an unsaturated bond may be contained in the organic group having a carbon number of 1 to 5. In addition, a fluorine atom may also be contained in the alkyl group.

[0098] By covering the surface of the silicon compound particles with a layer containing a compound having a silyl group such as a trialkylsilyl group, aggregation of the silicon compound particles is suppressed during electrode production, and water resistance is improved, thereby further improving the stability of the slurry.

[0099] Silyl groups such as alkylsilyl groups on the surface can be identified by TOF-SIMS. Detection of fragments of compounds having silyl groups such as alkylsilyl compounds on the outermost layer can be performed, for example, under the following conditions.

[0100] PHI TRIFT 2 manufactured by ULVAC-PHI,INCORPORATED.

[0101] Primary ion source: Gallium (Ga)

[0102] Sample temperature: 25°C

[0103] Accelerating voltage: 5kV

[0104] Focus spot size: 100μm×100μm

[0105] Sputtering: Ga, 100μm×100μm, 10s

[0106] Positive ion mass spectrometry

[0107] Sample: Indium metal powder molding

[0108] In addition, in the negative electrode active material of the present invention, the carbon material coverage is preferably 0.5 mass % or more and 15 mass % or less relative to the total of the silicon compound particles and the carbon material. If the carbon material coverage is such, a negative electrode active material particle with high capacity and excellent conductivity can be obtained.

[0109] In addition, in the negative electrode active material of the present invention, the volume resistivity of the negative electrode active material particles when 38.2 MPa is applied is preferably 0.01 Ω·cm or more and less than 100 Ω·cm as measured by the four-probe method based on JIS K7194. If the volume resistivity is 0.01 Ω·cm or more and less than 100 Ω·cm, sufficient conductivity can be ensured, so better battery characteristics can be obtained.

[0110] [Method for manufacturing negative electrode]

[0111] Next, an example of a method for producing a negative electrode of a nonaqueous electrolyte secondary battery of the present invention will be described.

[0112] First, a method for preparing a negative electrode material included in a negative electrode is described. First, a silicon compound (SiO x:0.5≤x≤1.6). Then, at least a portion of the silicon compound particles is covered with a carbon material. Then, the silicon compound particles are modified by absorbing lithium into the silicon compound particles. At this time, lithium compounds can be generated inside and on the surface of the silicon compound particles at the same time. In addition, at this time, a portion of the absorbed Li can be detached from the silicon compound particles. Then, a layer containing a compound having a silyl group is formed on the surface of the modified silicon compound particles or the surface of the carbon material or on at least a portion of the two surfaces. Then, the silicon compound particles formed with a layer containing a compound having a silyl group are used as negative electrode active material particles, and are mixed with a conductive aid and a binder, etc., so that a negative electrode material and a negative electrode can be manufactured.

[0113] More specifically, the negative electrode material can be produced, for example, through the following steps.

[0114] First, in the presence of an inert gas or under reduced pressure, a raw material for generating silicon oxide gas is heated in a temperature range of 900°C to 1600°C to generate silicon oxide gas. At this time, the raw material is a mixture of metal silicon powder and silicon dioxide powder. Considering the presence of oxygen on the surface of the metal silicon powder and trace amounts of oxygen in the reactor, the desired mixing molar ratio is in the range of 0.8 < metal silicon powder / silicon dioxide powder < 1.3. The Si crystallites in the particles are controlled by changing the feed range and the vaporization temperature, as well as the heat treatment after generation. The generated gas is deposited on an adsorption plate. The deposit is taken out while the temperature in the reactor is lowered to below 100°C, and is crushed and powdered using a ball mill, a jet mill, or the like.

[0115] Next, a carbon coating (carbon material) is formed on the surface of the obtained powder material (silicon compound particles). The carbon coating is effective in further improving the battery characteristics of the negative electrode active material.

[0116] As a method for forming a carbon film on the surface of the powder material, a pyrolysis CVD method is desirable. Pyrolysis CVD is to place silicon oxide powder in a furnace, fill the furnace with hydrocarbon gas, and raise the temperature in the furnace. The decomposition temperature is not particularly limited, but is particularly desirable to be below 1200°C. It is more desirable to be below 950°C to suppress unexpected disproportionation of silicon oxide. The hydrocarbon gas is not particularly limited, but is desirable to be C n H m The reason is that the production cost can be reduced and the physical properties of the decomposition product can be improved.

[0117] Next, the powder material is modified in its bulk. Examples of methods for modifying the bulk include electrochemical methods, redox methods, and thermal doping methods. The electrochemical method is preferably performed using a device that can electrochemically absorb and release Li. The device structure is not particularly limited, and for example, Figure 3 The in-body modification device 20 shown in the figure performs in-body modification. The in-body modification device 20 comprises: a bath 27 filled with an organic solvent 23; an anode electrode (lithium source, modification source) 21 disposed in the bath 27 and connected to one side of a power source 26; a powder storage container 25 disposed in the bath 27 and connected to the other side of the power source 26; and a diaphragm 24 provided between the anode electrode 21 and the powder storage container 25. Silicon oxide particles (silicon-based active material particles) 22 are contained in the powder storage container 25. In this way, silicon oxide particles are contained in the powder storage container, and a voltage is applied to the powder storage container containing silicon oxide particles and the anode electrode (lithium source) by the power source. As a result, lithium can be absorbed into the silicon compound particles or lithium can be separated from the silicon compound particles, so that the silicon oxide particles 22 can be modified. By heat-treating the obtained silicon oxide particles at 400 to 800° C., the Li compound can be stabilized. After modification, it can be cleaned with ethanol, alkaline water, weak acid or pure water.

[0118] As the organic solvent 23 in the bath 27, ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, fluoromethyl methyl carbonate, difluoromethyl methyl carbonate, etc. can be used. In addition, as the electrolyte salt contained in the organic solvent 23, lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), etc. can be used.

[0119] A lithium foil may be used as the anode electrode 21 , or a compound containing Li may be used. Examples of the compound containing Li include lithium carbonate, lithium oxide, lithium cobalt oxide, olivine-type lithium iron phosphate, lithium nickel oxide, and lithium vanadium phosphate.

[0120] In the modification based on the redox method, for example, first, lithium can be absorbed by immersing the silicon-based active material particles in a solution A in which lithium is dissolved in an ether solvent. The solution A may further contain a polycyclic aromatic compound or a linear polyphenyl compound. By heat-treating the obtained silicon-based active material particles at 400 to 800°C, the Li compound can be stabilized. In addition, after absorbing lithium, the active lithium can be separated from the silicon-based active material particles by immersing the silicon-based active material particles in a solution B containing a polycyclic aromatic compound or a derivative thereof. The solvent of the solution B can be, for example, an ether solvent, a ketone solvent, an ester solvent, an alcohol solvent, an amine solvent, or a mixed solvent of these solvents. After modification, it can be washed with ethanol, alkaline water, a weak acid or pure water.

[0121] As the ether solvent used for solution A, diethyl ether, tert-butyl methyl ether, tetrahydrofuran, dioxane, 1,2-dimethoxyethane, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether or a mixed solvent thereof can be used. Among them, tetrahydrofuran, dioxane, 1,2-dimethoxyethane and diethylene glycol dimethyl ether are particularly preferably used. These solvents are preferably dehydrated, and more preferably deoxygenated.

[0122] In addition, as the polycyclic aromatic compound contained in the solution A, naphthalene, anthracene, phenanthrene, tetraphenylene, pentylene, pyrene, triphenylene, coronene, and one or more derivatives of these polycyclic aromatic compounds. As the linear polyphenyl compound, biphenyl, terphenyl and one or more derivatives of these linear polyphenyl compounds can be used.

[0123] As the polycyclic aromatic compound contained in the solution B, naphthalene, anthracene, phenanthrene, tetraphenylene, pentylene, pyrene, triphenylene, coronene, and one or more derivatives of these polycyclic aromatic compounds.

[0124] Examples of the ether solvent of solution B include diethyl ether, tert-butyl methyl ether, tetrahydrofuran, dioxane, 1,2-dimethoxyethane, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, and mixed solvents of these ether solvents.

[0125] As the ketone solvent, acetone, acetophenone, or the like can be used.

[0126] As the ester solvent, methyl formate, methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, and the like can be used.

[0127] As the alcohol solvent, methanol, ethanol, propanol, isopropanol, etc. can be used.

[0128] As the amine solvent, methylamine, ethylamine, ethylenediamine, and the like can be used.

[0129] In the case of using a hot doping method for modification, for example, the powder material (silicon-based active material particles) can be mixed with LiH powder or Li powder and then heated in a non-oxidizing atmosphere to perform the modification. As a non-oxidizing atmosphere, for example, an Ar atmosphere can be used. More specifically, first, under an Ar atmosphere, the LiH powder or Li powder is fully mixed with the silicon oxide powder and then sealed, and the mixture is homogenized by stirring together with the sealed container. Then, the mixture is heated in a range of 700°C to 750°C and modified. In addition, at this time, in order to separate Li from the silicon compound particles, a method can be used in which the heated powder is fully cooled and then washed with ethanol or alkaline water, a weak acid or pure water.

[0130] Next, a layer containing a compound having a silyl group is formed on the surface of the modified silicon compound particles or the surface of the carbon material or at least a portion of the two surfaces. The layer containing the compound having a silyl group is preferably formed by treatment with an alkylsilazane. If in this way, a layer containing a compound having a silyl group can be effectively formed by treating the surface of the material. More specifically, for example, a layer containing a compound having a silyl group can be formed using the steps described below. In addition, it is believed that there is an OH group on the surface of the silicon compound particles or the carbon material, and the OH group reacts with the decomposition product of the alkylsilazane, whereby a trialkylsilyl group is introduced into the surface of the silicon compound particles or the carbon material.

[0131] First, dehydrated toluene, modified silicon compound particles of one quarter of the mass of dehydrated toluene, and HMDS (hexamethyldisilazane) equivalent to 3 mass % of the modified silicon compound particles were put into a container and stirred for 1 hour. Then, the silicon compound particles having a layer containing a compound having a silyl group formed thereon were filtered out as negative electrode active material particles.

[0132] Next, as needed, a silicon-based active material including silicon compound particles having the above-mentioned layer is mixed with a carbon-based active material, and these negative electrode active materials are mixed with other materials such as a binder and a conductive additive to prepare a negative electrode mixture, and then an organic solvent or water is added to prepare a slurry.

[0133] Then, if Figure 2 As shown, the negative electrode mixture slurry is applied to the surface of the negative electrode current collector 11 and dried to form the negative electrode active material layer 12. At this time, heating and pressing may be performed as needed. In the above manner, the negative electrode of the nonaqueous electrolyte secondary battery of the present invention can be manufactured.

[0134] <Lithium-ion secondary battery>

[0135] Next, the nonaqueous electrolyte secondary battery of the present invention is described. The nonaqueous electrolyte secondary battery of the present invention includes the negative electrode active material of the present invention. Here, as a specific example of the nonaqueous electrolyte secondary battery of the present invention, a laminated film type lithium ion secondary battery is described.

[0136] [Structure of laminated film type secondary battery]

[0137] Figure 4The laminated film type lithium ion secondary battery 30 shown mainly contains a wound electrode body 31 inside a sheet-like outer casing 35. The wound electrode body 31 has a separator between the positive electrode and the negative electrode and is wound. In addition, sometimes a separator is also provided between the positive electrode and the negative electrode and a laminate is contained. In any electrode body, a positive electrode lead 32 is attached to the positive electrode and a negative electrode lead 33 is attached to the negative electrode. The outermost peripheral portion of the electrode body is protected by a protective tape.

[0138] The positive and negative electrode leads 32 and 33 are led out in one direction from inside the exterior member 35 to the outside. The positive electrode lead 32 is made of a conductive material such as aluminum, and the negative electrode lead 33 is made of a conductive material such as nickel or copper.

[0139] The exterior member 35 is, for example, a laminated film in which a welding layer, a metal layer, and a surface protective layer are sequentially laminated, and the outer peripheral edges of the welding layers of two films are welded to each other or bonded with an adhesive or the like so that the welding layer faces the wound electrode body 31. The welding layer portion is, for example, a film of polyethylene or polypropylene, and the metal portion is, for example, aluminum foil. The protective layer is, for example, nylon or the like.

[0140] A close contact film 34 is inserted between the outer casing 35 and the positive and negative electrode leads to prevent the invasion of external gas. The material thereof is, for example, polyethylene, polypropylene, or polyolefin resin.

[0141] The positive electrode is for example Figure 2 The negative electrode 10 is the same as that of the positive electrode 10, and has a positive electrode active material layer on both sides or one side of the positive electrode collector.

[0142] The positive electrode current collector is formed of a conductive material such as aluminum.

[0143] The positive electrode active material layer includes any one or more of the positive electrode materials capable of absorbing and releasing lithium ions, and may also include other materials such as a positive electrode binder, a positive electrode conductive aid, and a dispersant according to the design. In this case, the details of the positive electrode binder and the positive electrode conductive aid are, for example, the same as those of the negative electrode binder and the negative electrode conductive aid described above.

[0144] The positive electrode material is preferably a compound containing lithium. Examples of the compound containing lithium include composite oxides composed of lithium and transition metal elements, or phosphate compounds containing lithium and transition metal elements. Among these positive electrode materials, compounds containing at least one of nickel, iron, manganese, and cobalt are preferred. As the chemical formula of these positive electrode materials, for example, Li x M1O2 or Li y M2PO4 represents. In the formula, M1 and M2 represent at least one transition metal element. The values ​​of x and y show different values ​​depending on the charge and discharge state of the battery, but are generally shown as 0.05≤x≤1.10 and 0.05≤y≤1.10.

[0145] As a composite oxide having lithium and a transition metal element, for example, a lithium cobalt composite oxide (Li x CoO2), a lithium nickel composite oxide (Li x NiO2), a lithium nickel cobalt composite oxide, etc. can be cited. As the lithium nickel cobalt composite oxide, for example, a lithium nickel cobalt aluminum composite oxide (NCA) and a lithium nickel cobalt manganese composite oxide (NCM), etc. can be cited.

[0146] As a phosphate compound having lithium and a transition metal element, for example, a lithium iron phosphate compound (LiFePO4) or a lithium iron manganese phosphate compound (LiFe 1-u Mn u PO4, (0 < u < 1)), etc. can be cited. If these cathode materials are used, a high battery capacity can be obtained, and at the same time, excellent cycle characteristics can also be obtained.

[0147] [Negative electrode]

[0148] The negative electrode has the same structure as the negative electrode 10 for the lithium ion secondary battery described above. For example, a negative electrode active material layer is provided on both sides of the current collector. Preferably, the negative electrode charging capacity of this negative electrode becomes larger than the capacitance obtained from the positive electrode active material (as the charging capacity of the battery). Thereby, the precipitation of lithium metal on the negative electrode can be suppressed. Figure 2 The positive electrode active material layer is provided on a part of both sides of the positive electrode current collector. Similarly, the negative electrode active material layer is also provided on a part of both sides of the negative electrode current collector. At this time, for example, the following region is provided: a region where the positive electrode active material layer opposite to the negative electrode active material layer provided on the negative electrode current collector does not exist. This is for stable battery design.

[0149] The region where the negative electrode active material layer and the positive electrode active material layer do not face each other is hardly affected by charge and discharge. Therefore, the state of the negative electrode active material layer can be maintained all the time after formation. Thereby, the composition of the negative electrode active material, etc. can be detected with good reproducibility and correctly without depending on whether there is charge and discharge.

[0150] The region where the negative electrode active material layer and the positive electrode active material layer do not face each other is hardly affected by charge and discharge. Therefore, the state of the negative electrode active material layer can be maintained all the time after formation. Thereby, the composition of the negative electrode active material, etc. can be detected with good reproducibility and correctly without depending on whether there is charge and discharge.

[0151] [Separator]

[0152] The separator isolates the positive electrode and the negative electrode, prevents current short - circuit due to contact between the two electrodes, and allows lithium ions to pass through. This separator is formed of, for example, a porous membrane composed of a synthetic resin or a ceramic, and may also have a laminated structure formed by laminating two or more porous membranes. As the synthetic resin, for example, polytetrafluoroethylene, polypropylene, polyethylene, etc. can be cited.

[0153] [Electrolyte solution]

[0154] At least a portion of the active material layer or the separator is impregnated with a liquid electrolyte (electrolyte solution). The electrolyte solution contains an electrolyte salt dissolved in a solvent and may contain other materials such as additives.

[0155] The solvent can use, for example, a non-aqueous solvent. As a non-aqueous solvent, for example, ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, 1,2-dimethoxyethane or tetrahydrofuran can be listed. Among them, it is desirable to use at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, and methyl ethyl carbonate. The reason is that better characteristics can be obtained. In addition, at this time, by combining high viscosity solvents such as ethylene carbonate and propylene carbonate with low viscosity solvents such as dimethyl carbonate, methyl ethyl carbonate, and diethyl carbonate, more advantageous characteristics can be obtained. The reason is that the dissociation and ion mobility of the electrolyte salt are improved.

[0156] As the solvent additive, it is preferred to include unsaturated carbon-bonded cyclic carbonate. The reason is that a stable coating will be formed on the negative electrode surface during charge and discharge, which can inhibit the decomposition reaction of the electrolyte. As the unsaturated carbon-bonded cyclic carbonate, for example, vinylene carbonate or vinyl ethylene carbonate etc. can be listed.

[0157] In addition, as a solvent additive, it is preferable to contain sultone (cyclic sulfonate) because it can improve the chemical stability of the battery. Examples of sultone include propane sultone and propene sultone.

[0158] Furthermore, the solvent preferably contains an acid anhydride. This is because the chemical stability of the electrolyte is improved. Examples of the acid anhydride include propane disulfonic acid anhydride.

[0159] The electrolyte salt may include at least one of light metal salts such as lithium salts. Examples of lithium salts include lithium hexafluorophosphate (LiPF6) and lithium tetrafluoroborate (LiBF4).

[0160] The content of the electrolyte salt is preferably 0.5 mol / kg to 2.5 mol / kg based on the solvent because high ion conductivity can be obtained.

[0161] [Method for producing laminated film type secondary battery]

[0162] Initially, the positive electrode is made using the above-mentioned positive electrode material. First, the positive electrode active material is mixed and the positive electrode binder, positive electrode conductive aid, etc. are mixed as needed to form a positive electrode mixture, which is then dispersed in an organic solvent to form a positive electrode mixture slurry. Next, the mixture slurry is applied to the positive electrode collector using a coating device such as a die coater with a knife roll or a die head, and the mixture slurry is dried with hot air to obtain a positive electrode active material layer. Finally, the positive electrode active material layer is compression molded using a roller press or the like. At this time, heating may be performed, and compression may also be repeated several times.

[0163] Subsequently, the negative electrode active material layer is formed on the negative electrode collector by the same operation procedure as that for producing the negative electrode 10 for the lithium ion secondary battery described above, thereby producing a negative electrode.

[0164] When manufacturing the positive electrode and the negative electrode, each active material layer is formed on both sides of the positive electrode collector and the negative electrode collector. At this time, the length of the active material coating on both sides of any electrode may be different (refer to Figure 2 ).

[0165] Next, prepare the electrolyte. Next, attach the positive electrode lead 32 to the positive electrode collector by ultrasonic welding or the like, and simultaneously attach the negative electrode lead 33 to the negative electrode collector. Next, stack or wind the positive electrode and the negative electrode through a separator to produce a wound electrode body 31, and adhere a protective tape to its outermost portion. Subsequently, the wound electrode body is formed in a flat shape. Next, after sandwiching the wound electrode body between the folded film-like outer packaging components 35, the insulating portions of the outer packaging components are bonded to each other by a thermal welding method, and the wound electrode body is sealed in a state open only in one direction. Next, insert a close-fitting film between the positive electrode lead and the negative electrode lead and the outer packaging component. Next, a prescribed amount of the above-prepared electrolyte is added from the open portion for vacuum impregnation. After impregnation, the open portion is bonded by a vacuum thermal welding method. In this way, a laminated film-type secondary battery 30 can be manufactured.

[0166] In the non-aqueous electrolyte secondary battery of the present invention such as the laminated film type secondary battery 30 produced above, the negative electrode utilization rate during charge and discharge is preferably 93% or more and 99% or less. If the negative electrode utilization rate is set in the range of 93% or more, the battery capacity can be greatly increased without reducing the initial charging efficiency. In addition, if the negative electrode utilization rate is set in the range of 99% or less, Li will not precipitate, and safety can be ensured.

[0167] Example

[0168] Hereinafter, although the Example and the comparative example of this invention are shown and this invention is demonstrated more concretely, this invention is not limited to these Examples.

[0169] (Example 1-1)

[0170] Follow these steps to make Figure 4 A laminated film type secondary battery 30 is shown.

[0171] First, the positive electrode was prepared. 95 parts by mass of the positive electrode active material, namely lithium nickel cobalt aluminum composite oxide (LiNi 0.7 Co 0.25 Al 0.05 O), 2.5 parts by mass of a positive electrode conductive aid (acetylene black), and 2.5 parts by mass of a positive electrode binder (polyvinylidene fluoride: PVDF) are mixed to form a positive electrode mixture. Next, the positive electrode mixture is dispersed in an organic solvent (N-methyl-2-pyrrolidone: NMP) to form a paste slurry. Next, a coating device with a die head is used to apply the slurry to both sides of the positive electrode collector, and a hot air drying device is used to dry it. At this time, a positive electrode collector with a thickness of 15 μm is used. Finally, compression molding is performed using a roller press.

[0172] Next, make a negative electrode. First, make a silicon-based active material in the following manner. A raw material (gasification starting material) mixed with metallic silicon and silicon dioxide is placed in a reactor, and the substance gasified in an atmosphere of 10Pa vacuum is deposited on an adsorption plate and fully cooled, and then the deposit is taken out and crushed using a ball mill. After adjusting the particle size, the carbon coating is covered by thermal CVD. Then, under an argon atmosphere, 4% by mass of LiH powder of silicon compound particles covered with carbon coating is mixed and stirred with a stirrer. Then, in an atmosphere-controlled furnace, the stirred powder is heat-treated at 740°C to modify it. Then, the modified silicon compound particles are put into a mixed solution in which 3% by mass of HMDS (hexamethyldisilazane) is dissolved in 2 times the amount of dehydrated toluene of the modified silicon compound particles, and stirred at room temperature for 1 hour. Then, the stirred silicon compound particles are filtered and dried to remove toluene. Thus, a layer containing a compound having a trimethylsilyl group is formed. The silicon-based active material is prepared in the above manner.

[0173] The silicon active material prepared in the above manner and the carbon active material were mixed at a mass ratio of 1:9 to prepare the negative electrode active material. Here, a mixture of natural graphite covered with an asphalt layer and artificial graphite at a mass ratio of 5:5 was used as the carbon active material. In addition, the median particle size of the carbon active material was 20 μm.

[0174] Next, the prepared negative electrode active material, conductive aid 1 (carbon nanotube, CNT), conductive aid 2 (carbon particles with a median particle size of about 50nm), styrene-butadiene rubber (styrene-butadiene copolymer, hereinafter referred to as SBR), and carboxymethyl cellulose (hereinafter referred to as CMC) are mixed at a dry mass ratio of 92.5:1:1:2.5:3, and diluted with pure water to prepare a negative electrode mixture slurry. In addition, the above-mentioned SBR and CMC are negative electrode binders (negative electrode adhesive). Here, in order to determine the stability of the negative electrode mixture slurry, a part of the prepared negative electrode mixture slurry, in addition to being used for the preparation of secondary batteries, an additional 30g is taken out and stored at 20°C to confirm the gas generation after the preparation of the negative electrode mixture slurry.

[0175] In addition, electrolytic copper foil (15 μm thick) was used as the negative electrode current collector. Finally, the negative electrode mixture slurry was applied to the negative electrode current collector and dried at 100°C for 1 hour in a vacuum atmosphere. After drying, the deposition amount of the negative electrode active material layer per unit area on the negative electrode single side (also called area density) was 5 mg / cm 2 .

[0176] Next, as a solvent, fluoroethylene carbonate (FEC), ethylene carbonate (EC) and diethyl carbonate (DEC) are mixed, and an electrolyte salt (lithium hexafluorophosphate: LiPF6) is dissolved to prepare an electrolyte solution. At this time, the composition of the solvent is set to FEC:EC:DEC=1:2:7 in volume ratio, and the content of the electrolyte salt relative to the solvent is set to 1.0 mol / kg. Further, 1.5% by mass of vinylene carbonate (VC) is added to the obtained electrolyte solution.

[0177] Next, assemble the secondary battery in the following manner. Initially, ultrasonically weld the aluminum lead to one end of the positive electrode collector, and weld the nickel lead to the negative electrode collector. Then, stack the positive electrode, separator, negative electrode, and separator in sequence, and wind them in the long side direction to obtain a wound electrode body. Use PET protective tape to fix the end of the winding. Use the following 12μm laminated film as a separator, wherein the laminated film is formed by sandwiching a film with porous polyethylene as the main component with a film with porous polypropylene as the main component. Then, after sandwiching the electrode body between the outer packaging components, the outer peripheral portions except one side are heat-fused to each other to accommodate the electrode body inside. An aluminum laminated film stacked with nylon film, aluminum foil and polypropylene film is used as an outer packaging component. Then, the prepared electrolyte is injected from the opening, impregnated in a vacuum atmosphere, and then heat-fused to perform sealing.

[0178] The cycle characteristics and initial charge and discharge characteristics of the secondary battery manufactured in the above manner were evaluated.

[0179] The cycle characteristics are detected in the following manner. Initially, in order to stabilize the battery, two cycles of charge and discharge are performed at 0.2C in an atmosphere of 25°C, and the discharge capacity of the second cycle is measured. Next, charge and discharge are performed until the total number of cycles is 299 cycles, and the discharge capacity is measured each time. Finally, the discharge capacity of the 300th cycle obtained by charging and discharging at 0.2C is divided by the discharge capacity of the second cycle to calculate the capacity retention rate (hereinafter also referred to as the retention rate). In the general cycle, that is, from the 3rd cycle to the 299th cycle, charge and discharge are performed in a manner of charging 0.7C and discharging 0.5C.

[0180] In the case of checking the initial charge and discharge characteristics, the initial efficiency is calculated. At this time, a 2032-type button cell is assembled as a test cell.

[0181] As the negative electrode, a negative electrode made by the same steps as the electrode containing a silicon-based active material of the above-mentioned laminated film type secondary battery is used. As an electrolyte, an electrolyte made by the same steps as the electrolyte of the above-mentioned laminated film type secondary battery is used. As a counter electrode, a metal lithium foil with a thickness of 0.5 mm is used. In addition, as a diaphragm, polyethylene with a thickness of 20 μm is used. Then, after overlapping the bottom cover, lithium foil, and diaphragm of the 2032-type button battery, 150 mL of electrolyte is injected, and then the negative electrode and the spacer (thickness of 1.0 mm) are overlapped and 150 mL of electrolyte is injected, and then the spring and the cap of the button battery are assembled in sequence, and crimped using an automatic button battery crimping machine to produce a 2032-type button battery.

[0182] Next, the prepared 2032-type button battery was charged at a constant current density of 0.2 mA / cm 2 The battery was charged until it reached 0.0 V. At the stage where the voltage reached 0.0 V, the battery was charged at a constant voltage of 0.0 V until the current density reached 0.02 mA / cm 2 When discharging, the current is 0.2 mA / cm 2 The battery was discharged at a constant current density until the voltage reached 1.2 V. The initial efficiency was calculated by the formula: initial efficiency (%) = (initial discharge capacity / initial charge capacity) × 100. The atmosphere temperature was set to be the same as that in the case of measuring the cycle characteristics.

[0183] In addition, the TOF-SIMS analysis was performed on the trial sample (silicon-based active material), and the intensity of the TMS (trimethylsilyl) component relative to the intensity of the C3H5 component was measured.

[0184] (Comparative Example 1-1)

[0185] Evaluation of the cycle characteristics of the secondary battery and the like were performed in the same procedure as in Example 1-1 except that the formation of the carbon coating and the formation of the layer containing the compound having a silyl group were not performed.

[0186] (Comparative Example 1-2)

[0187] Evaluation of the cycle characteristics of the secondary battery and the like were performed in the same procedure as in Example 1-1 except that the layer containing the compound having a silyl group was not formed.

[0188] [Table 1]

[0189] SiO x x=1,D 50 =5μm, graphite (natural graphite: artificial graphite = 5:5) D 50 =20μm

[0190] SiO x Ratio 10 mass%, half value width 1.85°, crystallite size 4.6nm, Li2Si2O5, Li2SiO3

[0191] Modification method: thermal doping method, volume resistivity 0.3Ω·cm

[0192]

[0193] X1 to X3 in Table 1 represent the types of three alkyl groups possessed by the trialkylsilyl group.

[0194] As shown in Table 1, when the surface treatment based on HMDS was not performed (Comparative Examples 1-1 and 1-2), the intensity of the TMS component relative to the intensity of the C3H5 component was 0, and no TMS group existed on the surface. In contrast, in Example 1-1 in which the HMDS treatment was performed, the intensity of the TMS component relative to the intensity of the C3H5 component was confirmed, and the presence of the TMS group on the surface was confirmed.

[0195] In addition, when these powders were used to confirm gas generation and battery characteristics, as shown in Table 1, in the case of trimethylsilyl groups, there were no agglomerates. In addition, the surface coating based on the silyl group was hydrophobicized, thereby observing the effect of suppressing the generation of gas from the slurry. As a result, both the initial efficiency and the cycle maintenance rate were improved. In the case of no silyl group, the time until the slurry generated gas was short, and agglomerates were further generated, resulting in poor initial efficiency and cycle maintenance rate.

[0196] (Examples 2-1 to 2-4)

[0197] The evaluation of the cycle characteristics of the secondary battery and the like were carried out in the same manner as in Example 1-1 except that the Li doping amount was changed to change the type of lithium silicate.

[0198] [Table 2]

[0199] SiO x x=1,D 50 =5μm, graphite (natural graphite: artificial graphite = 5:5) D 50 =20μm

[0200] SiO x Ratio 10 mass%, half value width 1.85°, crystallite size 4.6nm,

[0201] The carbon material coverage is 5% by mass, containing trimethylsilyl groups

[0202] Modification method: thermal doping method, volume resistivity 0.3Ω·cm

[0203]

[0204] As shown in Table 2, no aggregates were observed in any of the lithium silicates, and good results were obtained in terms of gas generation. In addition, in the case of including a Li compound, good results were obtained in both the initial efficiency and the capacity retention rate.

[0205] (Examples 3-1 to 3-5)

[0206] The evaluation of the cycle characteristics of the secondary battery and the like were carried out in the same procedure as in Example 1-1 except that the coating amount of the carbon material (carbon coating layer) was changed.

[0207] [Table 3]

[0208] SiO x x=1,D 50 =5μm, graphite (natural graphite: artificial graphite = 5:5) D 50 =20μm

[0209] SiO x Ratio 10 mass%, half value width 1.85°, crystallite size 4.6nm,

[0210] Li2Si2O5, Li2SiO3, containing trimethylsilyl, modification method: thermal doping

[0211]

[0212] As shown in Table 3, when the carbon coverage is large, the discharge can be performed reliably due to good conductivity, and the initial efficiency is improved. This can also achieve a high maintenance rate. When the carbon coverage is more than 15 mass%, the capacity advantage of SiO becomes smaller, so it is not practical. On the other hand, due to the deterioration of conductivity, the carbon coverage is expected to be 0.5 mass% or more.

[0213] (Examples 4-1 to 4-2)

[0214] Evaluation of the cycle characteristics of the secondary battery and the like were carried out in the same manner as in Example 1-1 except that the modification method was changed to the redox method and the crystallite size of the silicon compound particles was changed.

[0215] In Examples 4-1 and 4-2, when the silicon compound particles covered with a carbon coating are modified by absorbing lithium through a redox method, first, the silicon compound particles covered with a carbon coating are immersed in a solution (solution A) in which lithium flakes and naphthalene, which is an aromatic compound, are dissolved in tetrahydrofuran (hereinafter referred to as THF). The solution A is prepared by dissolving naphthalene in a THF solvent at a concentration of 0.2 mol / L, and then adding 10% by mass of lithium flakes to the mixed solution of THF and naphthalene. In addition, when the silicon compound particles covered with a carbon coating are immersed, the solution temperature is set to 20°C and the immersion time is set to 20 hours. Then, the modified silicon compound particles are filtered out. Lithium is absorbed into the silicon compound particles by the above treatment.

[0216] Next, the obtained silicon compound particles were heat treated at 600° C. for 24 hours in an argon atmosphere to stabilize the Li compound.

[0217] Next, the stabilized silicon compound particles are washed and dried under reduced pressure. Next, the dried silicon compound particles are put into a mixed solution in which 3% by mass of HMDS is dissolved in dehydrated toluene twice the amount of the modified silicon compound particles, and stirred at room temperature for 1 hour. Then, the stirred silicon compound particles are filtered and dried to remove toluene. Thus, a layer containing a compound having a trimethylsilyl group is formed. In the above manner, a silicon-based active material is prepared.

[0218] [Table 4]

[0219] SiO x x=1,D 50 =5μm, graphite (natural graphite: artificial graphite = 5:5) D 50 =20μm

[0220] SiO x Ratio 10% by mass Li2Si2O5, Li2SiO3, containing trimethylsilyl

[0221]

[0222] As shown in Table 4, the cycle maintenance rate is greatly improved by reducing the crystallite size. This is believed to be because the expansion and contraction of silicon are alleviated due to the small crystallite size. In addition, even if the doping method is changed to redox doping, the trimethylsilyl group can suppress condensation and delay the number of days of gas generation.

[0223] (Examples 5-1 to 5-5)

[0224] In addition to changing the particle size of the silicon compound particles (D 50 ) and the modification method, the cycle characteristics of the secondary battery were evaluated in the same manner as in Example 1-1.

[0225] [Table 5]

[0226] SiO x x=1, graphite (natural graphite: artificial graphite=5:5) D 50 =20μm

[0227] SiO x Ratio 10 mass%, half value width 1.85°, crystallite size 4.6 nm

[0228] Li2Si2O5, Li2SiO3, containing trimethylsilyl, modification method: redox method

[0229]

[0230] If the particle size of the silicon compound particles containing SiO is too small, the surface area becomes too large, so in order to extend the number of days of gas generation, the particle size is more preferably 2 μm or more. By increasing the particle size to reduce the surface area, the number of days of gas generation can be delayed. In addition, since the side reactions in the battery are also suppressed, the initial efficiency and cycle maintenance rate are improved. On the other hand, when the particle size is too large, due to the large expansion and contraction of SiO during charging and discharging, block collapse may occur, so it is expected to be less than 20 μm.

[0231] The present invention is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any technical solutions having substantially the same structure and exerting the same functions and effects as the technical concept described in the claims of the present invention are included in the technical scope of the present invention.

Claims

1. A negative electrode for a non-aqueous electrolyte secondary battery, comprising a negative electrode active material layer, wherein the negative electrode for a non-aqueous electrolyte secondary battery is characterized in that: The negative electrode active material layer comprises a negative electrode active material for a non-aqueous electrolyte secondary battery including negative electrode active material particles. The negative electrode active material particles contain a silicon compound SiO x Silicon compound particles, in, 0.5≤x≤1.6, The silicon compound particles contain a Li compound, At least a portion of the silicon compound particles is covered with a carbon material, The surface of the silicon compound particle or the surface of the carbon material or at least a part of both surfaces is covered with a layer containing a compound having a trialkylsilyl group, wherein the trialkylsilyl group has an alkyl group having 1 to 5 carbon atoms, At least a portion of the silicon compound particles comprises a 4 SiO 4 , Li 2 SiO 3 , Li 2 Si 2 O 5 At least one of the above.

2. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1, It is characterized in that The coverage amount of the carbon material is 0.5 mass % or more and 15 mass % or less with respect to the total of the silicon compound particles and the carbon material.

3. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1, It is characterized in that The negative electrode active material particles have a volume resistivity of 0.01 Ω·cm or more and less than 100 Ω·cm when 38.2 MPa is applied as measured by a four-probe method in accordance with JIS K7194.

4. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1, It is characterized in that The half-value width (2θ) of the diffraction peak caused by the Si (111) crystal plane obtained by X-ray diffraction of the silicon compound particles is 1.2° or more, and the crystallite size corresponding to the crystal plane is 7.5 nm or less.

5. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1, It is characterized in that The silicon compound particles have a median particle size of 0.5 μm or more and 20 μm or less.

6. A non-aqueous electrolyte secondary battery, It is characterized in that A negative electrode for a non-aqueous electrolyte secondary battery comprising the negative electrode according to any one of claims 1 to 5.

7. An electronic device, It is characterized in that A nonaqueous electrolyte secondary battery according to claim 6.

8. An electric tool, It is characterized in that A nonaqueous electrolyte secondary battery according to claim 6.

9. An electric car, It is characterized in that A nonaqueous electrolyte secondary battery according to claim 6.

10. A power storage system, It is characterized in that A nonaqueous electrolyte secondary battery according to claim 6.

11. A method for producing a negative electrode for a non-aqueous electrolyte secondary battery, the method comprising producing a negative electrode having a negative electrode active material layer, the method comprising: Production of silicon compound SiO x The process of preparing silicon compound particles, wherein 0.5≤x≤1.6; A step of covering at least a portion of the silicon compound particles with a carbon material; The step of modifying the silicon compound particles by absorbing lithium into the silicon compound particles, wherein at least a portion of the silicon compound particles contains a selected from Li 4 SiO 4 , Li 2 SiO 3 , Li 2 Si 2 O 5 At least one of the following; and forming a layer containing a compound having a trialkylsilyl group on the surface of the modified silicon compound particles or the surface of the carbon material or at least a part of both surfaces, wherein the trialkylsilyl group has an alkyl group having 1 to 5 carbon atoms; and using the silicon compound particles having the layer containing the compound having a trialkylsilyl group as negative electrode active material particles, thereby preparing a negative electrode material for a non-aqueous electrolyte secondary battery containing negative electrode active material particles containing silicon compound particles, A negative electrode for a non-aqueous electrolyte secondary battery is manufactured using the prepared negative electrode material for a non-aqueous electrolyte secondary battery.