A method for preparing ruthenium catalyst
The preparation of ruthenium catalysts through one-step reduction method solves the problems of complex and time-consuming preparation process in the prior art, and achieves efficient and simple preparation of ruthenium catalysts, which improves the decomposition activity of hydrazine, and is suitable for industrial use.
Patent Information
- Application Number
- CN202211456847.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-21
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-11-21
AI Technical Summary
The existing ruthenium catalyst preparation method has a complex process and is time-consuming, with low preparation efficiency, making it difficult to meet the needs of industrial production.
A one-step reduction method is used to prepare the ruthenium catalyst. By adding a catalyst support and a polyol solvent to the ruthenium precursor solution, heating reduction and multiple washings are performed to obtain a highly supported and highly dispersed ruthenium catalyst.
The preparation process is simplified, the time is shortened, and the preparation efficiency is improved. The prepared ruthenium catalyst has better decomposition catalytic activity on hydrazine at room temperature, and is suitable for large-scale production.
Smart Images

Figure CN115770569B_ABST
Abstract
Description
Technical Field
[0001] The method relates to a catalyst synthesis method, in particular to a preparation method of a ruthenium catalyst. Background Art
[0002] Hydrogen is a renewable, pollution-free, high-energy-density energy source that has received extensive attention in fuel cells for hydrogen-powered vehicles. Hydrazine (N2H4) has a high hydrogen content (12.5%), and the byproducts of complete decomposition to produce hydrogen are only nitrogen and water. In the presence of an appropriate catalyst, hydrogen can be released under mild conditions, and carbon emissions are zero during the hydrogen production process, making it an ideal liquid-phase hydrogen storage material.
[0003] Currently, among all elements, iridium (Ir) is the most active catalyst for the decomposition of hydrazine. However, iridium is very rare and its reserves are low. If it is used on a large scale, the economic cost will be very high. Ruthenium (Ru) is relatively cheap and is currently considered to be the most likely candidate catalyst to replace iridium for liquid phase hydrogen storage.
[0004] The existing synthesis methods of high-loaded ruthenium catalysts are very complicated and usually require dozens of repeated impregnation processes. Jofre et al. (JBFJofre et al., Acta Astronautica 85 (2013) 41-50) prepared ruthenium catalysts by continuous impregnation. The specific steps are as follows: before each impregnation step, the metal precursor (Ru(acac)3) and the alumina support are dried at 393K for 12 hours; then, the catalyst is heated to room temperature and the primary vacuum is 10°C. -3 bar for 1 hour; after each impregnation, the obtained solid is dried under primary vacuum and ambient temperature for 1 hour; before the reduction process begins, He is introduced into the reduction reactor at 393K for 30 minutes, and then the solid is reduced at 673K under hydrogen flow for 2.5 hours, and this is repeated 19 times. The difference is that in the last (i.e., the 20th) impregnation, the solid will be reduced at 673K under hydrogen flow for 4 hours to obtain a ruthenium catalyst. This synthesis method is relatively complicated. At the same time, according to records, it takes a total of 343 hours to prepare a catalyst using this method, which is time-consuming and has low preparation efficiency. Therefore, this method is not conducive to promotion and use. At present, it is urgent to develop a new method for preparing ruthenium catalysts. Summary of the invention
[0005] The present invention provides a method for preparing a ruthenium catalyst, which mainly solves the technical problems of the existing method for preparing a ruthenium catalyst, such as a complicated process, a long time consumption and a low efficiency.
[0006] The present invention provides a method for preparing a ruthenium catalyst, which is special in that it comprises the following steps:
[0007] Step 1, adding a catalyst carrier to a ruthenium precursor solution, mixing evenly to obtain a mixed solution; the ruthenium precursor solution is a mixed solution of a ruthenium precursor salt and a polyol solvent, and the mass volume ratio of the ruthenium precursor salt to the polyol solvent is (2.19-10.36):1; the unit of the mass of the ruthenium precursor salt is g, and the unit of the corresponding polyol solvent volume is L;
[0008] Step 2, heating the mixed solution to perform a reduction reaction to obtain a mixture;
[0009] Step 3, washing the mixture obtained in step 2 multiple times to obtain a precipitate, and drying the precipitate to obtain a ruthenium catalyst.
[0010] Furthermore, in step 1, the ruthenium precursor salt is one of ruthenium chloride, ruthenium acetate, ruthenium acetylacetonate, and bis(cyclopentadienyl)ruthenium.
[0011] Furthermore, in step 1, the catalyst carrier is one of γ-Al2O3, CeO2, SiO2, ZrO2, TiO2, and molecular sieve (Zeolite), and the structure of the catalyst carrier is powdery.
[0012] Furthermore, in step 1, the polyol solvent is one of EG, DEG, TEG, oleylamine, and glycerol.
[0013] Furthermore, in step 1, 100 mL of polyol solvent is added to every 500 mg of the catalyst carrier.
[0014] Furthermore, in step 2, the temperature of the reduction reaction is 180°C to 290°C, and the time is 30-50 minutes.
[0015] Furthermore, step 3 specifically includes adding water to the mixture obtained in step 2, centrifuging, removing the polyol solvent in the mixture, obtaining a precipitate after multiple additions of water and centrifugation, drying the precipitate, and then obtaining a ruthenium catalyst; wherein the mass ratio of the first added water to the mass of the mixture is 4 to 4.5:1.
[0016] Furthermore, in step 3, the number of washings is N, where N≥3.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] 1. The preparation method of the present invention is simple and efficient. The ruthenium catalyst can be obtained by one-step reduction followed by washing and drying. There is no need for dozens of repeated impregnation processes. Compared with the existing synthesis method of ruthenium catalyst, it is simpler, takes less time and is more efficient.
[0019] 2. The ruthenium catalyst prepared by the preparation method of the present invention has better decomposition catalytic activity for hydrazine at room temperature and can be produced in large quantities to meet industrial use.
[0020] 3. The catalyst carrier used in the present invention is a powder structure. The catalyst carrier with this structure can load more active metals per unit mass of catalyst, has a larger specific surface area and higher activity. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The present invention provides a comparison chart of the gas generation curves of the ruthenium catalyst prepared in Example 3 of the preparation method of a ruthenium catalyst of the present invention and the ruthenium catalyst prepared in Comparative Example 1 when hydrazine is decomposed at room temperature.
[0022] Figure 2 This is a transmission electron microscope image of the ruthenium catalyst prepared in Example 1 of the method for preparing a ruthenium catalyst of the present invention. DETAILED DESCRIPTION
[0023] The present invention provides a method for preparing a ruthenium catalyst, which mainly uses polyols to reduce ruthenium ions to nanoparticles at a certain temperature and load them on a carrier, thereby synthesizing a highly loaded and highly dispersed ruthenium catalyst in one step. The specific reaction principle is as follows:
[0024] Ruthenium precursor salt + HO-CH2-CH2-O-CH2-CH2-OH (DEG)
[0025] →Ruthenium nanoparticles + precursor ligand + HO-CH2-CH2-O-CH2-COOH;
[0026] During the reaction, the ruthenium precursor salt is first adsorbed on the Al2O3 carrier, and the DEG molecule is dehydrogenated to obtain the reducing HO-CH2-CH2-O-CH2-CH2-O - , and attacks the central ruthenium ion of the ruthenium precursor salt, then transfers electrons to the ruthenium ion and reduces it to ruthenium metal, which is loaded on the Al2O3 carrier to form nanoparticles. The main components of the final catalyst are metal nanoparticles (ruthenium) and Al2O3 carrier.
[0027] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0028] Embodiment 1
[0029] Mix 591.3 mg of ruthenium acetylacetonate (Ru(acac)3), 500 mg of γ-Al2O3 and 100 ml of diethylene glycol (DEG) to obtain a mixed solution; after the mixed solution is placed at room temperature for 4 hours, it is heated at 220°C for 40 minutes to obtain 112 g of a mixture; 450 g of water is added to the mixture, centrifuged, and the polyol solvent in the mixture is removed to obtain 1200 mg of a mixture; 45 g of water is added and centrifuged to obtain 1120 mg of a mixture; 45 g of water is added and centrifuged to obtain 1100 mg of a precipitate; the precipitate is dried at 60°C for 12 hours to obtain 1090 mg of a ruthenium catalyst Ru / Al2O3.
[0030] Figure 2 This is a transmission electron microscope image of a ruthenium catalyst prepared by the method of the present invention. It can be seen from the image that the ruthenium nanoparticles in the ruthenium catalyst have good dispersion on γ-Al2O3.
[0031] In this embodiment, the ruthenium precursor salt used is ruthenium acetylacetonate, and in other embodiments, the ruthenium precursor salt can also be ruthenium chloride or ruthenium acetate or diocene ruthenium. The catalyst carrier uses γ-Al2O3, and in other embodiments, the catalyst carrier can also use CeO2 or SiO2 or ZrO2 or TiO2 or molecular sieve (Zeolite), and the structure of the catalyst carrier used in each embodiment is powdered, and the active metal that can be loaded on the unit mass catalyst is more, the specific surface area is larger, and the activity is higher. DEG is used as the polyol solvent, and one of EG, TEG, oleylamine, and glycerol can also be used in other embodiments.
[0032] The amount of ruthenium precursor salt used is determined by the loading amount of the catalyst carrier, specifically:
[0033] The loading amount of the catalyst carrier = the mass of ruthenium metal / (the mass of ruthenium metal+the mass of the catalyst carrier); wherein, the mass of ruthenium metal = (the mass of the ruthenium precursor salt×the relative atomic mass of the ruthenium metal) / the relative molecular mass of the ruthenium precursor salt.
[0034] Embodiment 2
[0035] Mix 230 mg of ruthenium acetylacetonate (Ru(acac)3), 500 mg of γ-Al2O3 and 100 ml of diethylene glycol (DEG) to obtain a mixed solution; after the mixed solution is left at room temperature for 4 hours, heat it at 220°C for 40 minutes to obtain 111.7 g of a mixture; add 447 g of water to the mixture, centrifuge it, remove the polyol solvent in the mixture, obtain 780 mg of the mixture, add 30 g of water, centrifuge it, obtain 760 mg of the mixture, add 30 g of water, centrifuge it, obtain 740 mg of a precipitate, and dry the precipitate at 60°C for 12 hours to obtain 730 mg of a ruthenium catalyst Ru / Al2O3.
[0036] Embodiment 3
[0037] 219 mg of ruthenium acetylacetonate (Ru(acac)3), 500 mg of γ-Al2O3 and 100 ml of triethylene glycol (TEG) were mixed to obtain a mixed solution; the mixed solution was placed at room temperature for 4 hours, and then heated at 290°C for 30 minutes to obtain 112.7 g of a mixture; 450 g of water was added to the mixture, and the mixture was centrifuged to remove the polyol solvent in the mixture to obtain 780 mg of the mixture, and then 30 g of water was added and centrifuged to obtain 760 mg of the mixture, and then 30 g of water was added and centrifuged to obtain 730 mg of a precipitate, and the precipitate was dried at 60°C for 12 hours to obtain 719 mg of a ruthenium catalyst Ru / Al2O3. Figure 1 As shown in Figure 2, the catalyst has an activity of 1809.7 mmol g for the decomposition of hydrazine. Ru - 1 h -1 .
[0038] Embodiment 4
[0039] Mix 1036 mg of ruthenium acetylacetonate (Ru(acac)3), 500 mg of γ-Al2O3 and 100 ml of triethylene glycol (TEG) to obtain a mixed solution; after the mixed solution is placed at room temperature for 4 hours, it is heated at 250°C for 50 minutes to obtain 113.5 g of a mixture; 455 g of water is added to the mixture, centrifuged, and the polyol solvent in the mixture is removed to obtain 1580 mg of a mixture, and 50 g of water is added and centrifuged to obtain 1560 mg of a mixture, and 50 g of water is added and centrifuged to obtain 1555 mg of a precipitate, and the precipitate is dried at 60°C for 12 hours to obtain 1536 mg of a ruthenium catalyst Ru / Al2O3.
[0040] Embodiment 5
[0041] Mix 763.5 mg of ruthenium acetylacetonate (Ru(acac)3), 500 mg of γ-Al2O3 and 100 ml of diethylene glycol (DEG) to obtain a mixed solution; after the mixture is placed at room temperature for 4 hours, it is heated at 220°C for 40 minutes to obtain 112 g of a mixture; 450 g of water is added to the mixture, centrifuged, and the polyol solvent in the mixture is removed to obtain 1300 mg of a mixture; 50 g of water is added to the mixture, centrifuged to obtain 1280 mg of a mixture; 50 g of water is added to the mixture, centrifuged to obtain 1270 mg of a precipitate; the precipitate is dried at 60°C for 12 hours to obtain 1263 mg of a ruthenium catalyst Ru / Al2O3.
[0042] Comparative Example 1
[0043] 199 mg of ruthenium acetylacetonate (Ru(acac)3) and 500 mg of γ-Al2O3 were mixed and dried at 393 K for 12 h, then heated at ambient temperature with a primary vacuum of 10 -3 bar for 1 hour to obtain a solid mixture. Before the first reduction reaction, He was introduced into the reactor at 393K for 30 minutes, and then the solid mixture was reduced at 673K under a hydrogen flow for 2.5 hours, and this was repeated 19 times. In the 20th time, the solid mixture was reduced at 673K under a hydrogen flow for 4 hours to obtain 680 mg of ruthenium catalyst powder.
[0044] Combination Figure 1 It can be seen from Example 3 and Comparative Example 1 that the decomposition activity of the ruthenium catalyst (Ru / Al2O3) prepared by the preparation method of the present invention for hydrazine is 4.1 times that of the iridium catalyst prepared by the multiple impregnation method for hydrazine, and the decomposition activity is also better.
[0045] Although the embodiments of the present invention have been shown and described above, it will be apparent to those skilled in the art that any changes or modifications to the above embodiments should be deemed to fall within the protection scope of the present invention as long as they are within the spirit of the present invention.
Claims
1. A use of a ruthenium catalyst in the decomposition of hydrazine, characterized in that: The preparation method of the ruthenium catalyst comprises the following steps: Step 1, adding a catalyst carrier to a ruthenium precursor solution, mixing evenly to obtain a mixed solution; the ruthenium precursor solution is a mixed solution of a ruthenium precursor salt and a polyol solvent, and the mass volume ratio of the ruthenium precursor salt to the polyol solvent is (2.19-10.36) g:1L; the structure of the catalyst carrier is a powder, and one of γ-Al2O3, CeO2, SiO2, ZrO2, TiO2, and a molecular sieve is selected; Step 2, placing the mixed solution at room temperature for 4 hours and then heating it to perform a reduction reaction to obtain a mixture; the temperature of the reduction reaction is 180° C. to 290° C., and the time is 30-50 minutes; Step 3, washing the mixture obtained in step 2 multiple times to obtain a precipitate, and drying the precipitate to obtain a ruthenium catalyst.
2. The use of a ruthenium catalyst in hydrazine decomposition according to claim 1, characterized in that: In step 1, the ruthenium precursor salt is one of ruthenium chloride, ruthenium acetate, ruthenium acetylacetonate, and bis(cyclopentadienyl)ruthenium.
3. The use of a ruthenium catalyst in hydrazine decomposition according to claim 2, characterized in that: In step 1, the polyol solvent is one of EG, DEG, TEG, and glycerol.
4. The use of a ruthenium catalyst in hydrazine decomposition according to claim 3, characterized in that: In step 1, 100 mL of polyol solvent was added to every 500 mg of the catalyst support.
5. Use of a ruthenium catalyst according to any one of claims 1 to 4 in the decomposition of hydrazine, characterized in that: Step 3 specifically comprises adding water to the mixture obtained in step 2, centrifuging, removing the polyol solvent in the mixture, obtaining a precipitate after multiple additions of water and centrifugation, drying the precipitate, and then obtaining a ruthenium catalyst; wherein the mass ratio of the first added water to the mass of the mixture is 4-4.5:
1.
6. The use of a ruthenium catalyst in hydrazine decomposition according to claim 5, characterized in that: In step 3, the number of washings is N, where N≥3.