A method for reducing the anisotropy of mechanical properties of additively manufactured high-strength titanium alloys

By adding iron powder to Ti-1Al-8V-5Fe alloy powder and performing powder bed electron beam additive manufacturing and preheating treatment, the problem of anisotropy of mechanical properties of titanium alloys was solved and the strength and mechanical properties of titanium alloys were improved. Isotropic, suitable for manufacturing high-strength parts.

CN115770878BActive Publication Date: 2024-10-25NORTHWEST INSTITUTE FOR NONFERROUS METAL RESEARCH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211500273.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-28
Publication Date
2024-10-25
Estimated Expiration
2042-11-28

AI Technical Summary

Technical Problem

Titanium alloys have large anisotropy in mechanical properties during the powder bed electron beam additive manufacturing process, which increases the difficulty of preparation and limits their wide application in aerospace and other fields.

Method used

By adding iron powder to Ti-1Al-8V-5Fe alloy powder to increase its growth limiting factor and solidification temperature range, promoting the formation of equiaxed crystals, and performing ball milling and preheating treatment through powder bed electron beam additive manufacturing technology, Distribute iron powder evenly, reduce the β/α transition temperature, and improve the strength and composition uniformity of titanium alloys.

Benefits of technology

It significantly improves the isotropy of the strength and mechanical properties of titanium alloys, significantly increases the tensile strength and yield strength in the horizontal direction, increases the elongation after fracture, and reduces the strength anisotropy value, making it suitable for the manufacture of high-strength parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115770878B_ABST
    Figure CN115770878B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for reducing the anisotropy of mechanical properties of high-strength titanium alloys manufactured by additive manufacturing, the method comprising: 1. adding iron powder to spherical Ti185 alloy powder for ball milling to obtain mixed powder; 2. drawing a three-dimensional model of the target product and processing it in layers, obtaining slice data and designing slice scanning data; 3. importing the slice data and slice scanning data into the equipment to load powder and level the forming base plate and preheat; 4. laying the powder layer and preheating; 5. melting scanning to form a single-layer solid sheet; 6. repeating the above process to form a powder bed electron beam additive manufacturing formed part to obtain a high-strength titanium alloy. The present invention adds iron powder to Ti185 alloy powder for powder bed electron beam additive manufacturing, thereby improving the growth limiting factor and solidification temperature interval value of the alloy, facilitating the formation of equiaxed crystals in the titanium alloy, improving the strength of the titanium alloy, and reducing the anisotropy of the mechanical properties of the titanium alloy. As a high-strength component, it has a wide range of applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of alloy material preparation, and in particular relates to a method for reducing the anisotropy of mechanical properties of additively manufactured high-strength titanium alloys. Background Art

[0002] Titanium alloys have the advantages of high specific strength, good biocompatibility, corrosion resistance, non-magneticity, and heat resistance, and have been widely used in the fields of biomedicine, aerospace, marine engineering, petrochemicals, etc. With the rapid development of the aerospace industry, conventional titanium alloy materials are difficult to meet its needs, so high-strength titanium alloys have come into people's sight.

[0003] Titanium alloys have poor thermal conductivity, high deformation resistance, narrow forging temperature range, and high affinity for oxygen, which make the preparation of titanium alloy samples difficult. Powder bed electron beam additive manufacturing, also known as electron beam selected area melting (SEBM), is an advanced manufacturing technology developed in the 1990s. It has the advantages of fast scanning speed, high vacuum environment without pollution, and low residual stress. It is particularly suitable for the direct forming of active metal materials such as titanium alloys.

[0004] Ti-1Al-8V-5Fe (Ti185) alloy is a metastable β titanium alloy with high tensile strength and shear strength. It is widely used in aviation fasteners and some parts with high strength requirements. In addition, compared with other metastable β titanium alloys, the alloy has a lower cost. However, when Ti185 alloy is formed by powder bed electron beam additive manufacturing, the alloy has a coarse columnar crystal structure along the forming direction, resulting in obvious anisotropy of the alloy's mechanical properties. This problem seriously restricts the large-scale development and promotion of powder bed electron beam additive manufacturing and its preparation of titanium alloys. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for reducing the anisotropy of mechanical properties of high-strength titanium alloys manufactured by additive manufacturing in view of the deficiencies of the above-mentioned prior art. The method prepares titanium alloy by powder bed electron beam additive manufacturing by adding iron powder to Ti185 alloy powder, thereby improving the growth restriction factor and solidification temperature range of the alloy, facilitating the formation of equiaxed crystals in the titanium alloy, and reducing the β / α transition temperature, promoting the precipitation of nano-α strengthening phases in the titanium alloy, thereby improving the strength of the titanium alloy and reducing the anisotropy of mechanical properties of the titanium alloy.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for reducing the anisotropy of mechanical properties of additively manufactured high-strength titanium alloy, characterized in that the iron content in Ti-1Al-8V-5Fe alloy, i.e. Ti185 alloy powder, is increased, and a high-strength titanium alloy with isotropic mechanical properties is prepared by powder bed electron beam additive manufacturing. The method comprises the following steps:

[0007] Step 1: adding iron powder to the spherical Ti185 alloy powder prepared by plasma rotating electrode atomization, and then ball milling with a planetary ball mill to obtain a mixed powder;

[0008] Step 2: Draw a three-dimensional model of the target product titanium alloy, and then perform layering processing, cut it into slices of equal thickness along the height direction of the three-dimensional model, and obtain slice data, and then design the internal scanning method and scanning path of each slice to obtain slice scanning data;

[0009] Step 3: import the slice data and slice scanning data obtained in step 2 into the powder bed electron beam additive manufacturing equipment, load the mixed powder obtained in step 1 into the powder box of the powder bed electron beam additive manufacturing equipment, then level the forming base plate and preheat the forming base plate, the preheating temperature of the forming base plate is 700° C. to 720° C.;

[0010] Step 4: Spread the mixed powder loaded into the powder box in step 3 on the preheated forming bottom plate to form a powder layer, and then preheat the powder layer. The preheating temperature of the powder layer is 700° C. to 720° C. The thickness of the powder layer is the same as the thickness of the slice layer cut in step 3;

[0011] Step 5: According to the slice data and slice scanning data imported into the powder bed electron beam additive manufacturing forming equipment in step 3, the preheated powder layer in step 4 is melt-scanned by an electron beam to form a single-layer solid sheet, and then the forming base plate is lowered, and the lowering height of the forming base plate is the same as the thickness of the sheet cut in step 4;

[0012] Step six, repeat the powder laying process and preheating process in step four and the melting scanning process and the forming base plate descending process in step five until each single layer of solid sheets is stacked layer by layer to form a powder bed electron beam additive manufacturing formed part, and then take out the forming base plate when the temperature is less than 100°C, and use high-pressure gas to remove residual powder on the surface of the powder bed electron beam additive manufacturing formed part to obtain a high-strength titanium alloy; the high-strength titanium alloy has a tensile strength in the horizontal direction higher than 1317MPa, a tensile strength in the vertical direction higher than 1303MPa, a tensile yield strength in the horizontal direction higher than 1241MPa, a tensile yield strength in the vertical direction higher than 1222MPa, an elongation after fracture higher than 5%, and a strength anisotropy value not higher than 1.5.

[0013] The present invention uses spherical Ti185 alloy powder prepared by plasma rotating electrode atomization as raw material and adds iron powder for ball milling and mixing to obtain mixed powder, and then prepares high-strength titanium alloy with isotropic mechanical properties through powder bed electron beam additive manufacturing. First, the spherical Ti185 alloy powder prepared by plasma rotating electrode atomization used in the present invention has high sphericity and a particle size suitable for powder bed electron beam additive manufacturing equipment. The spherical powder is easy to spread evenly during the additive manufacturing process, which is beneficial to improving the uniformity of the structure of the Ti185 alloy; secondly, the present invention increases the growth limiting factor and solidification temperature range of the alloy by adding iron powder to the spherical Ti185 alloy powder, which is beneficial to the formation of equiaxed crystals. At the same time, iron is a β-stabilizing element, and the increase in iron content reduces the β / α transition temperature of the alloy. Preparation combined with powder bed electron beam additive manufacturing is beneficial to the titanium alloy to obtain a finer strengthening phase α and reduce the anisotropy of the mechanical properties of the titanium alloy; and the spherical Ti185 alloy powder and iron powder are ball milled in a planetary ball mill Mixing is beneficial to the uniform distribution of iron powder on the surface of Ti185 alloy powder, which is beneficial to improving the composition uniformity of the product titanium alloy; thirdly, in the powder bed electron beam additive manufacturing process of the present invention, by preheating the forming base plate and the powder layer, and controlling the preheating temperature to 700°C ~ 720°C, each prepared single-layer solid sheet is subjected to repeated heat treatment processes, which is beneficial to the gradual release of thermal stress inside the product titanium alloy, and then the internal structure of the titanium alloy tends to be uniform. At the same time, the spherical Ti185 alloy powder of the powder layer is first preheated and then melt-scanned, so that adhesion occurs between the powders, avoiding the movement of the powder layer caused by the impact of the electron beam, improving the interlayer bonding strength of the titanium alloy, and avoiding the occurrence of component segregation of the titanium alloy, especially the segregation of the Fe element to produce β spot defects, affecting the strength of the titanium alloy.

[0014] The above-mentioned method for reducing the anisotropy of mechanical properties of high-strength titanium alloys manufactured by additive manufacturing is characterized in that the spherical Ti185 alloy powder in step one is composed of the following components by mass content: Al 1.38%, V 8.00%, Fe4.22%, O 0.19%, and the balance is titanium and unavoidable impurities, and the particle size of the spherical Ti185 alloy powder is 40μm to 150μm. The spherical Ti185 alloy powder of this particle size has good fluidity, which is conducive to the spreading of the mixed powder on the forming bottom plate, improves the uniformity of the powder layer, and then improves the uniformity of each component in the product titanium alloy, avoiding the occurrence of component segregation; at the same time, the spherical Ti185 alloy powder of this particle size is conducive to improving its melting rate in the powder bed electron beam additive manufacturing process.

[0015] The above-mentioned method for reducing the anisotropy of mechanical properties of additively manufactured high-strength titanium alloys is characterized in that the particle size of the iron powder in step one is 1 μm, and the amount added is 1.89% of the mass of the spherical Ti185 alloy powder. By controlling the particle size of the iron powder, it is beneficial for the iron powder to adhere evenly to the surface of the Ti185 alloy powder and not to agglomerate. Generally, the iron mass content of the Ti185 alloy is 4% to 6%. According to the chemical element ratio calculation method, 1.89% iron powder is added to the Ti185 alloy powder of the present invention to prepare a mixed powder. The iron content in the mixed powder is still within the component content range of the conventional Ti185 alloy powder, avoiding the introduction of other impurity elements, which is beneficial to ensure the mechanical properties of the titanium alloy.

[0016] The ball milling process of the present invention is as follows: iron powder is added to the spherical Ti185 alloy powder prepared by plasma rotating electrode atomization, and then the powder is placed in a ball milling jar of a planetary ball mill, and ball milling beads and ethanol are added to the ball milling jar, and the powder is ball milled for 4 hours at a rotation speed of 20 r / min to obtain a mixed powder. In the process, ethanol is added to promote the iron powder to be uniformly attached to the surface of the spherical Ti185 alloy powder.

[0017] The above-mentioned method for reducing the anisotropy of mechanical properties of additively manufactured high-strength titanium alloy is characterized in that the thickness of the equal-thickness layer in step 2 is 0.1 mm. The thickness of the layer is controlled to be 0.1 mm to adapt to the melting ability of the electron beam on the mixed powder.

[0018] The above-mentioned method for reducing the anisotropy of mechanical properties of high-strength titanium alloys manufactured by additive manufacturing is characterized in that the process parameters of the melting scan in step 5 are: scanning line spacing 0.1mm, scanning current 15mA, scanning speed 3300mm / s. The above-mentioned melting scanning forming parameters are used to perform powder bed electron beam additive manufacturing of titanium alloy on titanium alloy spherical powder, which effectively controls the dimensional accuracy and melting quality of each layer during the forming process, so that the prepared titanium alloy formed part is uniform inside and has a complete shape, which is conducive to improving the strength of the titanium alloy.

[0019] Compared with the prior art, the present invention has the following advantages:

[0020] 1. The present invention prepares titanium alloy by adding iron powder to Ti185 alloy powder for powder bed electron beam additive manufacturing, thereby improving the growth limitation factor and solidification temperature range of the alloy, which is beneficial to the formation of equiaxed crystals in the titanium alloy, while reducing the β / α transition temperature and promoting the precipitation of nano-α strengthening phase in the titanium alloy, thereby improving the strength of the titanium alloy and reducing the anisotropy of the mechanical properties of the titanium alloy.

[0021] 2. The present invention adds iron powder to Ti185 alloy powder and controls the addition amount according to the chemical element ratio calculation method, which not only promotes the formation of equiaxed crystals in the titanium alloy, but also ensures that the iron content in the mixed powder after addition is within the component content range of conventional Ti185 alloy powder, avoiding the introduction of other impurity elements, which is beneficial to ensuring the mechanical properties of the titanium alloy.

[0022] 3. In the powder bed electron beam additive manufacturing process of the present invention, the powder layer and the forming base plate are preheated, which is beneficial to the gradual release of thermal stress inside the product titanium alloy, so that the internal structure of the titanium alloy tends to be uniform, while avoiding adhesion between powders, improving the bonding strength between titanium alloy layers and avoiding component segregation, further ensuring the strength and other mechanical properties of the titanium alloy.

[0023] 4. The present invention adds iron powder and combines it with powder bed electron beam additive manufacturing, so that the interior of the prepared titanium alloy is equiaxed crystal, high strength and significantly reduces the anisotropy of mechanical properties, the tensile strength in the horizontal direction is higher than 1317MPa, the tensile strength in the vertical direction is higher than 1303MPa, the tensile yield strength in the horizontal direction is higher than 1241MPa, the tensile yield strength in the vertical direction is higher than 1222MPa, the elongation after fracture is higher than 5%, and the strength anisotropy value is not higher than 1.5. It can be made into high-strength components with a wide range of applications.

[0024] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is an optical microscope image of the titanium alloy prepared in Example 1 of the present invention.

[0026] Figure 2 This is an optical microscope image of the titanium alloy prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0027] The powder bed electron beam additive manufacturing equipment used in Examples 1-2 of the present invention and Comparative Examples 1-2 is a Sialon Y150 model.

[0028] Example 1

[0029] This embodiment includes the following steps:

[0030] Step 1, put 1kg of spherical Ti185 alloy powder with a particle size of 40μm to 150μm prepared by plasma rotating electrode atomization into a ball mill, then add 18.9g of iron powder with a particle size of 1μm, then add ball milling beads and ethanol, and use a planetary ball mill to perform ball milling at a speed of 20r / min for 4h to obtain a mixed powder; the spherical Ti185 alloy powder consists of the following components by mass content: Al 1.38%, V 8.00%, Fe 4.22%, O 0.19%, and the balance is titanium and unavoidable impurities;

[0031] Step 2: Use Magics software to draw a three-dimensional model of the target product titanium alloy, the model size is 80mm×13mm×22mm (length×width×height), and then perform layering processing, cut it into equal-thickness slices with a thickness of 0.1mm along the height direction of the three-dimensional model, and obtain slice data, and then design the internal scanning method and scanning path of each slice to obtain slice scanning data; the slice scanning data includes: scanning line spacing of 0.1mm, scanning current of 15mA, and scanning speed of 3300mm / s;

[0032] Step 3: Import the slice data and slice scanning data obtained in step 2 into the powder bed electron beam additive manufacturing equipment, load 8 kg of the mixed powder obtained in step 1 into the powder box of the powder bed electron beam additive manufacturing equipment, and then level the forming base plate and preheat the forming base plate. The preheating temperature of the forming base plate is 720° C., and the size of the forming base plate is 100 mm×100 mm×10 mm (length×width×thickness);

[0033] Step 4: Spread the mixed powder loaded into the powder box in step 3 on the preheated forming base plate to form a powder layer with a thickness of 0.1 mm, and then preheat the powder layer at a preheating temperature of 720° C.

[0034] Step 5: According to the slice data and slice scanning data imported into the powder bed electron beam additive manufacturing forming equipment in step 3, the preheated powder layer in step 4 is melt-scanned by an electron beam to form a single-layer solid sheet, and then the forming base plate is lowered by 0.1 mm; the process parameters of the melt scanning are: scanning line spacing 0.1 mm, scanning current 15 mA, scanning speed 3300 mm / s;

[0035] Step six, repeat the powder laying process and preheating process in step four and the melting scanning process and forming base plate lowering process in step five until each single layer of solid sheets is stacked layer by layer to form a powder bed electron beam additive manufacturing molded part, and then take out the forming base plate when the temperature is less than 100°C, and use high-pressure gas to remove residual powder on the surface of the powder bed electron beam additive manufacturing molded part to obtain a high-strength titanium alloy.

[0036] After testing, the high-strength titanium alloy prepared in this embodiment has a horizontal tensile strength of 1336MPa, a tensile yield strength of 1270MPa, and an elongation of 9%, a vertical tensile strength of 1366MPa, a tensile yield strength of 1256MPa, and an elongation of 6%, a tensile strength anisotropy of 1.4, and a tensile yield strength anisotropy of 1.1. The anisotropy value (IPA) is calculated according to formula (1).

[0037]

[0038] In formula (1), T H Indicates the tensile or yield strength of the specimen in the horizontal direction, in MPa; T V It indicates the tensile or yield strength of the specimen in the vertical direction, in MPa.

[0039] Figure 1 This is an optical microscope image of the titanium alloy prepared in this embodiment. Figure 1 It can be seen that the titanium alloy is equiaxed crystal along the forming direction, with fine α phase inside.

[0040] Comparative Example 1

[0041] The difference between this comparative example and Example 1 is that this comparative example does not have step 1, that is, iron powder is not added to the Ti185 alloy powder to obtain the Ti185 alloy.

[0042] After testing, the Ti185 alloy prepared in this comparative example has a tensile strength of 1075 MPa in the horizontal direction, a tensile yield strength of 1005 MPa, and an elongation of 17%; a tensile strength of 1131 MPa in the vertical direction, a tensile yield strength of 1059 MPa, and an elongation of 6%; an anisotropy value of tensile strength is 5.1, and an anisotropy value of tensile yield strength is 5.2.

[0043] Figure 2 The optical microscope image of the titanium alloy prepared in this comparative example is Figure 2 It can be seen that the titanium alloy has a columnar crystal structure along the forming direction.

[0044] Comparing Example 1 with Comparative Example 1, it can be seen that the growth restriction factor and solidification temperature interval of the Ti185 alloy powder without iron powder in Comparative Example 1 are relatively low. After calculation, the growth restriction factor of the Ti185 alloy (iron content of 4.22%) is 46.8, and the solidification temperature interval is 96°C; while in Example 1, 1.89% iron powder is added to the Ti185 alloy powder to form a mixed titanium alloy powder, and the growth restriction factor of the titanium alloy (iron content of 6%) is 66.6, and the solidification temperature interval is 129°C. According to the interdependence theory of solidification, the higher the growth restriction factor and the solidification temperature interval, the easier it is to form equiaxed crystals. Therefore, the interior of the titanium alloy obtained in Example 1 is equiaxed crystals, while the interior of the titanium alloy obtained in Comparative Example 1 is columnar crystals, and the grain size and the size of the strengthening phase in the crystal are smaller than those of the corresponding columnar crystals, resulting in the former having higher strength than the latter.

[0045] Comparative Example 2

[0046] The difference between this comparative example and Example 1 is that: in step 1 of this comparative example, the amount of iron powder added is 41.1 g, and the mass content of iron in the titanium alloy is 8%.

[0047] In the forming process of the powder bed electron beam additive manufacturing used in this comparative example, the powder fluidity was poor and a large amount of splashing was generated during the forming process, resulting in the termination of the forming process.

[0048] Comparing Example 1 with Comparative Example 2, it can be seen that the amount of iron powder added in Comparative Example 2 is 4.11%, and the mass content of iron in the titanium alloy is as high as 8%. Due to the excessively high content of iron powder, the sphericity of the mixed powder deteriorates, thereby reducing fluidity. At the same time, since the melting point of iron differs from that of the Ti185 alloy by more than 100°C, when the mass content of iron powder increases, a large amount of splashing is generated during the forming process using the powder bed electron beam additive manufacturing technology, which seriously affects the performance of the formed part and causes the forming process to fail.

[0049] In summary, the present invention improves the growth limitation factor and solidification temperature range of the alloy by adding iron powder to Ti185 alloy powder and controlling the amount of iron powder added to 6%. At the same time, the mixed powder has good fluidity to ensure the progress of the forming process and promote the formation of equiaxed crystals in the titanium alloy, thereby improving the strength of the titanium alloy.

[0050] Example 2

[0051] This embodiment includes the following steps:

[0052] Step 1, put 1kg of spherical Ti185 alloy powder with a particle size of 40μm to 150μm prepared by plasma rotating electrode atomization into a ball mill, then add 18.9g of iron powder with a particle size of 1μm, then add ball milling beads and ethanol, and use a planetary ball mill to perform ball milling at a speed of 20r / min for 4h to obtain a mixed powder; the spherical Ti185 alloy powder consists of the following components by mass content: Al 1.38%, V 8.00%, Fe 4.22%, O 0.19%, and the balance is titanium and unavoidable impurities;

[0053] Step 2: Use Magics software to draw a three-dimensional model of the target product titanium alloy, the model size is 80mm×13mm×22mm (length×width×height), and then perform layering processing, cut it into equal-thickness slices with a thickness of 0.1mm along the height direction of the three-dimensional model, and obtain slice data, and then design the internal scanning method and scanning path of each slice to obtain slice scanning data; the slice scanning data includes: scanning line spacing of 0.1mm, scanning current of 15mA, and scanning speed of 3300mm / s;

[0054] Step 3: Import the slice data and slice scanning data obtained in step 2 into the powder bed electron beam additive manufacturing equipment, load 8 kg of the mixed powder obtained in step 1 into the powder box of the powder bed electron beam additive manufacturing equipment, and then level the forming base plate and preheat the forming base plate. The preheating temperature of the forming base plate is 700° C., and the size of the forming base plate is 100 mm×100 mm×10 mm (length×width×thickness);

[0055] Step 4: Spread the mixed powder loaded into the powder box in step 3 on the preheated forming base plate to form a powder layer with a thickness of 0.1 mm, and then preheat the powder layer at a preheating temperature of 700° C.

[0056] Step 5: According to the slice data and slice scanning data imported into the powder bed electron beam additive manufacturing forming equipment in step 3, the preheated powder layer in step 4 is melt-scanned by an electron beam to form a single-layer solid sheet, and then the forming base plate is lowered by 0.1 mm; the process parameters of the melt scanning are: scanning line spacing 0.1 mm, scanning current 15 mA, scanning speed 3300 mm / s;

[0057] Step six, repeat the powder laying process and preheating process in step four and the melting scanning process and forming base plate lowering process in step five until each single layer of solid sheets is stacked layer by layer to form a powder bed electron beam additive manufacturing molded part, and then take out the forming base plate when the temperature is less than 100°C, and use high-pressure gas to remove residual powder on the surface of the powder bed electron beam additive manufacturing molded part to obtain a high-strength titanium alloy.

[0058] After testing, the high-strength titanium alloy prepared in this embodiment has a tensile strength of 1317 MPa in the horizontal direction, a tensile yield strength of 1241 MPa, and an elongation at break of 7%; a tensile strength of 1303 MPa in the vertical direction, a tensile yield strength of 1222 MPa, and an elongation at break of 5%, an anisotropy value of tensile strength of 1.1, and an anisotropy value of tensile yield strength of 1.5.

[0059] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for reducing the anisotropy of mechanical properties of additively manufactured high-strength titanium alloys, characterized in that: By increasing the iron content in Ti-1Al-8V-5Fe alloy, i.e., Ti185 alloy powder, a high-strength titanium alloy with isotropic mechanical properties is prepared by powder bed electron beam additive manufacturing, the method comprising the following steps: Step 1: adding iron powder to the spherical Ti185 alloy powder prepared by plasma rotating electrode atomization, and then ball milling with a planetary ball mill to obtain a mixed powder; Step 2: Draw a three-dimensional model of the target product titanium alloy, and then perform layering processing, cut it into slices of equal thickness along the height direction of the three-dimensional model, and obtain slice data, and then design the internal scanning method and scanning path of each slice to obtain slice scanning data; Step 3: import the slice data and slice scanning data obtained in step 2 into the powder bed electron beam additive manufacturing equipment, load the mixed powder obtained in step 1 into the powder box of the powder bed electron beam additive manufacturing equipment, then level the forming base plate and preheat the forming base plate, the preheating temperature of the forming base plate is 700° C. to 720° C.; Step 4: Spread the mixed powder loaded into the powder box in step 3 on the preheated forming bottom plate to form a powder layer, and then preheat the powder layer. The preheating temperature of the powder layer is 700° C. to 720° C. The thickness of the powder layer is the same as the thickness of the slice layer cut in step 3; Step 5: According to the slice data and slice scanning data imported into the powder bed electron beam additive manufacturing forming equipment in step 3, the preheated powder layer in step 4 is melt-scanned by an electron beam to form a single-layer solid sheet, and then the forming base plate is lowered, and the lowering height of the forming base plate is the same as the thickness of the sheet cut in step 4; Step six, repeat the powder laying process and preheating process in step four and the melting scanning process and the forming base plate descending process in step five until each single layer of solid sheets is stacked layer by layer to form a powder bed electron beam additive manufacturing formed part, and then take out the forming base plate when the temperature is less than 100°C, and use high-pressure gas to remove residual powder on the surface of the powder bed electron beam additive manufacturing formed part to obtain a high-strength titanium alloy; the high-strength titanium alloy has a tensile strength in the horizontal direction higher than 1317MPa, a tensile strength in the vertical direction higher than 1303MPa, a tensile yield strength in the horizontal direction higher than 1241MPa, a tensile yield strength in the vertical direction higher than 1222MPa, an elongation after fracture higher than 5%, and a strength anisotropy value not higher than 1.

5.

2. A method for reducing the anisotropy of mechanical properties of additively manufactured high-strength titanium alloy according to claim 1, characterized in that: The spherical Ti185 alloy powder in step 1 is composed of the following components by mass content: Al 1.38%, V 8.00%, Fe 4.22%, O 0.19%, and the remainder is titanium and unavoidable impurities, and the particle size of the spherical Ti185 alloy powder is 40 μm to 150 μm.

3. The method for reducing the anisotropy of mechanical properties of additively manufactured high-strength titanium alloy according to claim 1, characterized in that: The particle size of the iron powder in step 1 is 1 μm, and the added amount is 1.89% of the mass of the spherical Ti185 alloy powder.

4. The method for reducing the anisotropy of mechanical properties of additively manufactured high-strength titanium alloy according to claim 1, characterized in that: The thickness of the equal-thickness sheet in step 2 is 0.1 mm.

5. The method for reducing the anisotropy of mechanical properties of additively manufactured high-strength titanium alloy according to claim 1, characterized in that: The process parameters of the melting scan in step 5 are: scanning line spacing 0.1 mm, scanning current 15 mA, and scanning speed 3300 mm / s.