Silicone sealant for photovoltaic modules resistant to moisture and heat aging and preparation method and application thereof

By adding MQ silicone resin and modified fillers to the silicone sealant, combined with the mixing process under vacuum conditions, the problem of the mechanical properties of the silicone sealant declining after moisture and heat aging is solved, and effective sealing and sealing of solar photovoltaic modules are achieved. Encapsulation.

CN115772382BActive Publication Date: 2024-10-18HUBEI XINGRUI SILICON MATERIAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211501263.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-28
Publication Date
2024-10-18
Estimated Expiration
2042-11-28

AI Technical Summary

Technical Problem

The existing silicone sealant's mechanical properties and mechanical property retention rate deteriorate after 1,000 hours of double 85 moisture-heat aging, resulting in bonding failure and inability to effectively seal and encapsulate solar photovoltaic modules.

Method used

Using a one-component silicone sealant formula, including α,ω-dihydroxypolydimethylsiloxane, MQ silicone resin, modified fillers, cross-linking agents, catalysts and hydroxyl scavengers, through mixing and mixing under vacuum conditions Prepared by dispersion process, MQ silicone resin, modified filler and hydroxyl scavenger are added to improve the tensile strength and tensile strength retention rate initially and after moist heat aging.

Benefits of technology

Significantly improves the initial tensile strength, tensile strength and tensile strength retention rate of the silicone sealant after moist heat aging, and maintains good elasticity after moist heat aging, solving the problem of bonding failure, and is suitable for solar photovoltaic modules sealing and encapsulation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003967766550000071
    Figure BDA0003967766550000071
Patent Text Reader

Abstract

The present invention provides a silicone sealant for a photovoltaic module resistant to damp heat aging, and a preparation method and application thereof, wherein the sealant comprises the following raw materials in parts by weight: 100 parts of α, ω-dihydroxy polydimethylsiloxane, 10-30 parts of a plasticizer, 1-10 parts of an MQ silicone resin, 100-200 parts of a filler, 1-15 parts of a modified filler, 5-15 parts of a cross-linking agent, 2-4 parts of a coupling agent, 1-2 parts of a catalyst, and 1-10 parts of a hydroxyl scavenger; wherein the modified filler is silane-modified calcium chloride and / or magnesium chloride. By adding MQ silicone resin, modified filler, and hydroxyl scavenger, the product still has good tensile strength, elasticity, and tensile strength retention after 1000 hours of double 85 damp heat aging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of silicone rubber, and specifically relates to a silicone sealant for a moisture-heat-aging-resistant photovoltaic module and a preparation method and an application method thereof. Background Art

[0002] Room temperature vulcanized silicone sealant is widely used in construction, electronics, aerospace, automotive industry, medicine and health, new energy and other fields due to its excellent bonding and sealing properties, non-corrosiveness to substrates, ability to maintain good physical and electrical properties in harsh environments, and ease of use.

[0003] Since solar cells have physical and chemical defects such as thinness, brittleness, and easy oxidation, long-term exposure to natural conditions such as air and rain can easily cause permanent damage, making it difficult to apply solar power generation on a large scale under harsh natural conditions. Therefore, to achieve the industrial application of solar power generation, it is required to seal and encapsulate it. This sealing and encapsulation is a key technology for achieving industrial production and large-scale application of photovoltaic power generation. The application environment of adhesive for solar photovoltaic modules is mainly outdoors, which puts forward the following performance requirements for its performance: good weather resistance, able to withstand erosion such as severe cold, heat, strong winds and rainstorms; good adhesion (under ultraviolet radiation, heavy rain, strong winds, high and low temperature environments), that is, silicone sealant products are required to still have good tensile strength, elasticity and tensile strength retention rate after 1000 hours of double 85 wet heat aging. Summary of the invention

[0004] The present invention provides a silicone sealant for a moisture-heat aging resistant photovoltaic module and a preparation method and application thereof, which solves the problems that the mechanical properties and mechanical property retention rate of the existing silicone sealant products deteriorate after 1000 hours of double 85 moisture-heat aging, resulting in bonding failure, thereby making it impossible to seal and package the solar photovoltaic module.

[0005] The technical solution of the present invention is a single-component silicone sealant for moisture-heat aging resistant photovoltaic modules, which comprises the following raw materials in parts by weight: 100 parts of α, ω-dihydroxy polydimethylsiloxane, 10-30 parts of plasticizer, 1-10 parts of MQ silicone resin, 100-200 parts of filler, 1-15 parts of modified filler, 5-15 parts of cross-linking agent, 2-4 parts of coupling agent, 1-2 parts of catalyst and 1-10 parts of hydroxyl scavenger; wherein the modified filler is silane-modified calcium chloride and / or magnesium chloride.

[0006] Furthermore, the viscosity of the α,ω-dihydroxypolydimethylsiloxane at 25° C. is 20000-100000 mPa·s.

[0007] Furthermore, the plasticizer is one or more of dimethyl silicone oil, phenyl silicone oil, hydrogen silicone oil or amino silicone oil, and has a viscosity of 100-1500 mPa·s at 25°C.

[0008] Furthermore, the MQ silicone resin is a mixture of MQ resin and silicone oil in a mass ratio of 1-2:5-10, wherein the molar ratio of M to Q segments in the MQ resin is 0.60:1-0.90:1; and the MQ resin is one or more of methyl MQ resin, methyl phenyl MQ resin or phenyl MQ resin.

[0009] Furthermore, the filler is formed by mixing nano calcium carbonate, fumed silica and silicon powder in a ratio of 80-200:0-10:0-50; wherein the nano calcium carbonate is modified by stearic acid, aluminate coupling agent, borate coupling agent or silane coupling agent, and the particle size of the filler is 40-100 nm.

[0010] Furthermore, the particle size of the modified filler is below 100 μm, wherein the moisture content is less than 5 wt%; the silane is one or more of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, epoxypropyltriethoxysilane and mercaptopropyltrimethoxysilane; the mass ratio of calcium chloride and / or magnesium chloride to silane is 1 to 3:10.

[0011] Furthermore, the hydroxyl scavenger is at least one of hexamethyldisilazane, tetramethyldivinyldisilazane, diphenyltetramethyldisilazane, and hexaphenylcyclotrisilazane.

[0012] Furthermore, the crosslinking agent is at least one of methyl tributylacetoxime siloxane, vinyl tributylacetoxime siloxane, phenyl tributylacetoxime siloxane, tetrabutyl ketone oxime siloxane, dimethyl dibutyl ketone oxime siloxane, and methyl vinyl dibutyl ketone oxime siloxane.

[0013] Furthermore, the coupling agent is at least one of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, and N-(2-aminoethyl)-3-aminopropyltriethoxysilane; and the catalyst is at least one of dibutyltin diacetate, dibutyltin dilaurate, dibutyltin diacetylacetonate, and dibutyltin diacetylacetate.

[0014] The present invention also relates to a method for preparing the silicone sealant, comprising the following steps:

[0015] S1. Put α, ω-dihydroxy polydimethylsiloxane and plasticizer into a kneader and mix them evenly. The vacuum degree is -0.08 to -0.1 MPa. Dehydrate at 100-120°C. Then add fillers and modified fillers and disperse them evenly to obtain a basic rubber compound.

[0016] S2. Add MQ resin, crosslinking agent, coupling agent and catalyst to the material obtained in S1, and disperse them evenly under the condition of vacuum degree of -0.08 to -0.1 MPa. Then add hydroxyl scavenger to the material, and disperse and mix them evenly under the condition of vacuum degree of -0.08 to -0.1 MPa to obtain a single-component silicone sealant for moisture-heat aging resistant photovoltaic modules.

[0017] The invention also relates to the application of the one-component silicone sealant for moisture-heat-aging-resistant photovoltaic modules in the bonding of solar photovoltaic modules.

[0018] The present invention has the following beneficial effects:

[0019] By adding MQ silicone resin, modified filler and hydroxyl scavenger, the initial tensile strength of the product, the tensile strength after wet heat aging and the tensile strength retention rate are improved, and the sample can maintain good elasticity after wet heat aging. The organic part in MQ silicone resin can improve its compatibility with silicone rubber, and the siloxane chain energy can improve the mechanical strength, cohesive strength, peel strength and high temperature and humidity resistance of silicone rubber. Calcium chloride and / or magnesium chloride are added to effectively absorb moisture in the rubber material to prevent the methyl groups on the molecular chain from being oxidized and degraded under the action of oxygen after moisture enters, resulting in the breakage of the silicone rubber molecular chain; at the same time, silane is used to modify it to improve the compatibility of calcium chloride and / or magnesium chloride with terminal hydroxyl polysiloxane, so that it can be more evenly dispersed in the base glue. Hexamethyldisilazane and calcium chloride were compounded for trial use. Since hexamethyldisilazane was added alone, it would react with hydroxyl and moisture to produce a weakly alkaline substance ammonia during storage, and calcium chloride can absorb ammonia, further improving the storage stability and wet heat aging resistance of the sealant.

[0020] The silicone sealant for the moisture-heat-aging resistant photovoltaic module provided by the present invention is designed as a single component, is easy to use, and can be widely used in the sealing and packaging of solar photovoltaic modules. DETAILED DESCRIPTION

[0021] The embodiments of the present invention will be described in detail below with reference to examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention.

[0022] Embodiment 1:

[0023] 100 parts of 20000mPa·sα,ω-dihydroxy polydimethylsiloxane, 10 parts of dimethyl silicone oil, 100 parts of sodium stearate modified nano calcium carbonate, 1 part of fumed silica, and 10 parts of silicon micropowder are put into a kneader and mixed evenly, and dehydrated at 100-120°C for 180min with a vacuum degree of -0.08MPa, and a basic rubber material is obtained after the high-temperature dehydration is completed;

[0024] Add 2 parts of methyl MQ silicone resin (the molar ratio of M to Q segments is 0.6:1) to the planetary machine, stir and disperse for 30 minutes at a vacuum degree of -0.1MPa, add the base rubber after mixing evenly, stir and disperse for 30 minutes at a vacuum degree of -0.1MPa, add 9 parts of methyl tributyl ketoxime silane, 3 parts of vinyl tributyl ketoxime silane, 2 parts of KH-550, and 1 part of dibutyltin dilaurate to the planetary machine, stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. Add 1 part of hexamethyldisilazane to the planetary machine, stir and disperse for 30 minutes at a vacuum degree of -0.1MPa, and the sealant product is obtained.

[0025] Embodiment 2:

[0026] 100 parts of 20000mPa·sα,ω-dihydroxypolydimethylsiloxane, 10 parts of dimethyl silicone oil, 90 parts of stearic acid-modified nano-calcium carbonate, 1 part of fumed silica, 10 parts of silicon micropowder and 10 parts of modified calcium chloride are put into a kneader and mixed evenly, and dehydrated at high temperature for 180 minutes, with a vacuum degree of -0.08MPa and a temperature of 100-120°C, to obtain a basic rubber material after the high-temperature dehydration is completed; the preparation method of the modified calcium chloride is as follows: 100 parts of calcium chloride powder are placed in a high-speed stirrer for stirring and dispersing for 30 minutes, and after the dispersion is completed, 10 parts of a modifier N-(2-aminoethyl)-3-aminopropyltrimethoxysilane are weighed, and the high-speed stirring and dispersion is continued for 2 hours and then sealed and stored to obtain the modified calcium chloride powder.

[0027] Add 2 parts of methyl MQ silicone resin (the molar ratio of M to Q segments is 0.6:1) to the planetary machine, stir and disperse for 30 minutes at a vacuum degree of -0.1MPa, add the base rubber after mixing evenly, and stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. Add 9 parts of methyl trisbutyl ketoxime silane, 3 parts of vinyl trisbutyl ketoxime silane, 2 parts of KH-550, and 1 part of dibutyltin dilaurate to the planetary machine, stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. Add 1 part of hexamethyldisilazane to the planetary machine, stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. The sealant product is obtained.

[0028] Example 3

[0029] 100 parts of 20000mPa·sα,ω-dihydroxypolydimethylsiloxane, 10 parts of dimethyl silicone oil, 90 parts of stearic acid-modified nano-calcium carbonate, 1 part of fumed silica, 10 parts of silicon micropowder and 10 parts of modified magnesium chloride are put into a kneader and mixed evenly, and dehydrated at high temperature for 180 minutes, with a vacuum degree of -0.08MPa and a temperature of 100-120°C, and a basic rubber material is obtained after the high-temperature dehydration is completed; the preparation method of the modified magnesium chloride is as follows: 100 parts of calcium chloride powder are placed in a high-speed stirrer for stirring and dispersing for 30 minutes, and after the dispersion is completed, 10 parts of a modifier N-(2-aminoethyl)-3-aminopropyltrimethoxysilane are weighed, and the high-speed stirring and dispersing is continued for 2 hours, and then the modified magnesium chloride powder is sealed and stored.

[0030] Add 2 parts of methyl MQ silicone resin (the molar ratio of M to Q segments is 0.6:1) to the planetary machine, stir and disperse for 30 minutes at a vacuum degree of -0.1MPa, add the base rubber after mixing evenly, and stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. Add 9 parts of methyl trisbutyl ketoxime silane, 3 parts of vinyl trisbutyl ketoxime silane, 2 parts of KH-550, and 1 part of dibutyltin dilaurate to the planetary machine, stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. Add 1 part of hexamethyldisilazane to the planetary machine, stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. The sealant product is obtained.

[0031] Example 4

[0032] Put 100 parts of 20000mPa·sα,ω-dihydroxy polydimethylsiloxane, 10 parts of dimethyl silicone oil, 90 parts of stearic acid-modified nano calcium carbonate, 1 part of fumed silica, 10 parts of silicon micropowder and 10 parts of modified calcium chloride into a kneader and mix them evenly, and dehydrate them at high temperature for 180 minutes at a vacuum degree of -0.1MPa and a temperature of 100-120°C to obtain a basic rubber material after the high temperature dehydration is completed;

[0033] Add 2 parts of methyl MQ silicone resin (the molar ratio of M to Q segments is 0.4:1) to the planetary machine, stir and disperse for 30 minutes at a vacuum degree of -0.1MPa, add the base rubber after mixing evenly, and stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. Add 9 parts of methyl tributylidene oxime silane, 3 parts of vinyl tributylidene oxime silane, 2 parts of KH-550, and 1 part of dibutyltin dilaurate to the planetary machine, and stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. Add 1 part of hexamethyldisilazane to the planetary machine, and stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. The sealant product can be obtained.

[0034] Example 5

[0035] Put 100 parts of 20000mPa·sα,ω-dihydroxy polydimethylsiloxane, 10 parts of dimethyl silicone oil, 90 parts of stearic acid-modified nano calcium carbonate, 1 part of fumed silica, 10 parts of silicon micropowder and 10 parts of modified calcium chloride into a kneader and mix them evenly, and dehydrate them at high temperature for 180 minutes at a vacuum degree of -0.08 to -0.1MPa and a temperature of 100-120°C to obtain a basic rubber material after high temperature dehydration is completed;

[0036] Add 2 parts of methyl MQ silicone resin (the molar ratio of M to Q segments is 0.96:1) to the planetary machine, stir and disperse for 30 minutes at a vacuum degree of -0.1MPa, add the base rubber after mixing evenly, and stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. Add 9 parts of methyl trisbutyl ketoxime silane, 3 parts of vinyl trisbutyl ketoxime silane, 2 parts of KH-550, and 1 part of dibutyltin dilaurate to the planetary machine, stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. Add 1 part of hexamethyldisilazane to the planetary machine, stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. The sealant product can be obtained.

[0037] Example 6

[0038] 100 parts of 20000mPa·sα,ω-dihydroxypolydimethylsiloxane, 10 parts of dimethyl silicone oil, 100 parts of stearic acid-modified nano-calcium carbonate, 1 part of fumed silica and 10 parts of silicon micropowder were put into a kneader and mixed evenly. The mixture was dehydrated at high temperature for 180 minutes at a vacuum degree of -0.1MPa and a temperature of 100-120°C. After the high-temperature dehydration was completed, the basic rubber material was obtained.

[0039] Add 9 parts of methyl tributylidene oxime silane, 3 parts of vinyl tributylidene oxime silane, 2 parts of KH-550, and 1 part of dibutyltin dilaurate into a planetary machine containing the base rubber, and stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. Add 1 part of hexamethyldisilazane into the planetary machine, and stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. The sealant product can be obtained.

[0040] Example 7

[0041] Put 100 parts of 20000mPa·sα,ω-dihydroxy polydimethylsiloxane, 10 parts of dimethyl silicone oil, 90 parts of stearic acid-modified nano calcium carbonate, 1 part of fumed silica, 10 parts of silicon micropowder and 10 parts of unmodified calcium chloride into a kneader and mix them evenly, and dehydrate them at high temperature for 180min, with a vacuum degree of -0.08MPa and a temperature of 100-120°C, to obtain a basic rubber material after the high temperature dehydration is completed;

[0042] Add 2 parts of methyl MQ silicone resin (the molar ratio of M to Q segments is 0.6:1) to the planetary machine, stir and disperse for 30 minutes at a vacuum degree of -0.1MPa, add the base rubber after mixing evenly, and stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. Add 9 parts of methyl trisbutyl ketoxime silane, 3 parts of vinyl trisbutyl ketoxime silane, 2 parts of KH-550, and 1 part of dibutyltin dilaurate to the planetary machine, stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. Add 1 part of hexamethyldisilazane to the planetary machine, stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. The sealant product can be obtained.

[0043] Example 8

[0044] Put 100 parts of 20000mPa·sα,ω-dihydroxypolydimethylsiloxane, 10 parts of dimethyl silicone oil, 90 parts of stearic acid-modified nano-calcium carbonate, 1 part of fumed silica, 10 parts of silicon micropowder and 10 parts of unmodified calcium chloride into a kneader and mix evenly, dehydrate at high temperature for 180 minutes with a vacuum degree of -0.08MPa and a temperature of 100-120°C, and obtain the basic rubber material after the high-temperature dehydration is completed.

[0045] Add 9 parts of methyl tributylidene oxime silane, 3 parts of vinyl tributylidene oxime silane, 2 parts of KH-550, and 1 part of dibutyltin dilaurate into a planetary machine containing the base rubber, and stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. Add 1 part of hexamethyldisilazane into the planetary machine, and stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. The sealant product can be obtained.

[0046] Example 9

[0047] 100 parts of 20000mPa·sα,ω-dihydroxypolydimethylsiloxane, 10 parts of dimethyl silicone oil, 90 parts of stearic acid-modified nano-calcium carbonate, 1 part of fumed silica, 10 parts of silicon micropowder and 10 parts of modified calcium chloride are put into a kneader and mixed evenly, and dehydrated at high temperature for 180 minutes at a vacuum degree of -0.08MPa and a temperature of 100-120°C. After the high-temperature dehydration is completed, a basic rubber material is obtained; wherein the average particle size of the nano-calcium carbonate is 50nm.

[0048] Add 2 parts of methyl MQ silicone resin to the planetary machine, stir and disperse for 30 minutes at a vacuum degree of -0.1MPa, add the base rubber after mixing evenly, and stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. Add 9 parts of methyl tributylidene oxime silane, 3 parts of vinyl tributylidene oxime silane, 2 parts of KH-550, and 1 part of dibutyltin dilaurate to the planetary machine, and stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. Stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. The sealant product can be obtained.

[0049] Example 10

[0050] 100 parts of 2000mPa·sα,ω-dihydroxypolydimethylsiloxane, 15 parts of amino silicone oil, 90 parts of nano calcium carbonate modified by silane coupling agent, 10 parts of fumed silica, 50 parts of silicon micropowder and 10 parts of modified calcium chloride were put into a kneader and mixed evenly, and dehydrated at high temperature for 180min, with a vacuum degree of -0.08MPa and a temperature of 100-120°C. After the high temperature dehydration is completed, a basic rubber material is obtained; the preparation of modified calcium chloride is the same as in Example 2.

[0051] Add 10 parts of methyl MQ silicone resin (the molar ratio of M to Q segments is 0.8:1) to the planetary machine, stir and disperse for 30 minutes at a vacuum degree of -0.1MPa, add the base rubber after mixing evenly, and stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. Add 5 parts of vinyl trisbutyl ketone oxime siloxane, 10 parts of phenyl trisbutyl ketone oxime siloxane, 4 parts of N-(2-aminoethyl)-3-aminopropyl trimethoxysilane, and 2 parts of dibutyltin diacetate to the planetary machine, stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. Add 5 parts of tetramethyl divinyl disilazane to the planetary machine, stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. The sealant product is obtained.

[0052] Embodiment 11

[0053] 100 parts of 5000mPa·sα,ω-dihydroxypolydimethylsiloxane, 10 parts of phenyl silicone oil, 150 parts of nano calcium carbonate modified by borate coupling agent, 10 parts of silicon powder and 10 parts of modified calcium chloride were put into a kneader and mixed evenly, and dehydrated at high temperature for 180min, with a vacuum degree of -0.09MPa and a temperature of 100-120°C. After the high temperature dehydration is completed, a basic rubber material is obtained; the preparation of modified calcium chloride is the same as in Example 2.

[0054] Add 5 parts of methyl MQ silicone resin (the molar ratio of M to Q segments is 0.8:1) to the planetary machine, stir and disperse for 30 minutes at a vacuum degree of -0.1MPa, add the base rubber after mixing evenly, and stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. Add 10 parts of tetrabutyl ketone oxime siloxane, 3 parts of N-(2-aminoethyl)-3-aminopropyl triethoxysilane, and 1 part of dibutyltin diacetylacetonate to the planetary machine, and stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. Add 10 parts of hexaphenylcyclotrisilazane to the planetary machine, and stir and disperse for 30 minutes at a vacuum degree of -0.1MPa. The sealant product is obtained.

[0055] The performance test results of the above embodiment are shown in Table 1. The testing standard is the national standard GB / T 29595-2013 "Silicone rubber sealant for ground photovoltaic module sealing material".

[0056] Table 1

[0057]

[0058]

[0059] It can be seen from the results in Table 1 that the comparison results of Example 2 and Example 6 show that the initial tensile strength of the product, the tensile strength after wet heat aging, and the tensile strength retention rate are improved by adding MQ silicone resin, modified calcium chloride, and hexamethyldisilazane, and the sample can maintain good elasticity after wet heat aging. Among them, the comparison results of Example 2 and Example 3 show that modified magnesium chloride can effectively improve the wet heat aging resistance of the sample. Comparing Example 1 with Example 2, the initial mechanical properties and mechanical properties after wet heat aging and the mechanical property retention rate of the product are improved by adding modified calcium chloride and hexamethyldisilazane, and the sample can also maintain good elasticity after wet heat aging. Comparing Example 2 with Example 7, unmodified calcium chloride is used as filler, and its compatibility with the base glue is poor, the powder is easy to agglomerate and cannot be evenly dispersed in the base glue, resulting in poor initial mechanical properties and mechanical properties after wet heat aging. Comparing Example 2 with Example 9, the compounding trial of hexamethyldisilazane and calcium chloride has the best effect. Since hexamethyldisilazane is added alone, it will react with hydroxyl and moisture to produce a weak alkaline substance ammonia during storage, and calcium chloride can absorb ammonia, further improving the storage stability and resistance to wet heat aging of the sealant. In summary, the compounding trial of MQ silicone resin, modified calcium chloride and hexamethyldisilazane can effectively improve the initial tensile strength of the product, the tensile strength after wet heat aging, and the tensile strength retention rate, and the sample can maintain good elasticity after wet heat aging.

[0060] The above embodiments describe the preferred implementation of the present invention, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A one-component silicone sealant for photovoltaic modules resistant to moisture and heat aging, characterized in that: The invention comprises the following raw materials in parts by weight: 100 parts of α, ω-dihydroxy polydimethylsiloxane, 10-30 parts of plasticizer, 1-10 parts of MQ silicone resin, 100-200 parts of filler, 1-15 parts of modified filler, 5-15 parts of crosslinking agent, 2-4 parts of coupling agent, 1-2 parts of catalyst and 1-10 parts of hydroxyl scavenger hexamethyldisilazane; wherein the modified filler is silane-modified calcium chloride and / or magnesium chloride; the MQ silicone resin is methyl The invention discloses a MQ silicone resin, wherein the molar ratio of M to Q segments is 0.60:1-0.90:1; the filler is prepared by mixing nano calcium carbonate, fumed silica and silicon powder in a ratio of 80-200:0-10:0-50, and the nano calcium carbonate is modified by stearic acid, aluminate coupling agent, borate coupling agent or silane coupling agent; and the viscosity of α,ω-dihydroxy polydimethylsiloxane at 25°C is 20000-100000 mPa•s.

2. The silicone sealant according to claim 1, characterized in that: The plasticizer is one or more of dimethyl silicone oil, phenyl silicone oil, hydrogen silicone oil or amino silicone oil, and has a viscosity of 100-1500 mPa•s at 25°C.

3. The silicone sealant according to claim 1, characterized in that: The filler particle size is 40 to 100 nm.

4. The silicone sealant according to claim 1, characterized in that: The particle size of the modified filler is below 100 μm, wherein the moisture content is less than 5wt%; the silane is one or more of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-βaminoethylγ-aminopropyltrimethoxysilane, N-βaminoethylγ-aminopropyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, epoxypropyltriethoxysilane and mercaptopropyltrimethoxysilane; the mass ratio of calcium chloride and / or magnesium chloride to silane is 1-3:

10.

5. The silicone sealant according to claim 1, characterized in that: The crosslinking agent is at least one of methyl tributylacetoximine siloxane, vinyl tributylacetoximine siloxane, phenyl tributylacetoximine siloxane, tetrabutyl ketone oxime siloxane, dimethyl dibutyl ketone oxime siloxane, and methyl vinyl dibutyl ketone oxime siloxane.

6. The silicone sealant according to claim 1, characterized in that: The coupling agent is at least one of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, and N-(2-aminoethyl)-3-aminopropyltriethoxysilane; and the catalyst is at least one of dibutyltin diacetate, dibutyltin dilaurate, dibutyltin diacetylacetonate, and dibutyltin diacetylacetate.

7. The method for preparing the silicone sealant according to any one of claims 1 to 6, characterized in that: The specific steps are: S1. Put α, ω-dihydroxy polydimethylsiloxane and plasticizer into a kneader and mix them evenly. The vacuum degree is -0.08 to -0.1 MPa. Dehydrate at 100-120°C. Then add fillers and modified fillers and disperse them evenly to obtain a basic rubber compound. S2. Mix the MQ resin and add the material obtained in S1 and mix again. Then add the cross-linking agent, coupling agent and catalyst, and disperse them evenly under the condition of vacuum degree of -0.08 to -0.1MPa. Finally, add the hydroxyl scavenger to the material, and disperse and mix them evenly under the condition of vacuum degree of -0.08 to -0.1MPa to obtain a single-component silicone sealant for moisture-heat aging resistant photovoltaic modules.

8. Use of the one-component silicone sealant for moisture-heat-aging-resistant photovoltaic modules according to any one of claims 1 to 6 in bonding solar photovoltaic modules.

Citation Information

Patent Citations

  • Single-component silicone sealant for automobile lamp and preparation method of single-component silicone sealant

    CN102627940A

  • Ageing resistant type solar photovoltaic component sealing material and preparation method thereof

    CN104277759A