A method and device for on-site remanufacturing of large pile legs of marine engineering equipment

By using pile movement system and laser remelting technology on pile legs of marine engineering equipment, the problem of on-site repair of pile legs is solved, efficient material utilization and repair layer performance improvement is achieved, and the pile legs is significantly improved Stability and safety.

CN115772640BActive Publication Date: 2024-11-05GUANGDONG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211450901.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-18
Publication Date
2024-11-05
Estimated Expiration
2042-11-18

AI Technical Summary

Technical Problem

Large pile legs of marine engineering equipment are damaged by corrosion and wear in the marine environment, resulting in the impact of stability and safety. The existing technology lacks effective on-site in-situ repair methods and equipment.

Method used

Adopt pile movement system, robot, laser three-dimensional scanning detection system, X-ray flaw detector, spray control system and laser remelting system. By thermal spraying of metal coating and laser remelting and laser forging, the damaged area is gradually repaired and the internal one is eliminated. Defect and restore the original design dimensions.

Benefits of technology

It effectively reduces heat input, improves material utilization, eliminates pores, enhances the bonding strength and wear resistance of the repair layer, and reduces the repair cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115772640B_ABST
    Figure CN115772640B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for on-site in-situ remanufacturing of large pile legs of marine engineering equipment. The method adopts the methods of thermal spraying pre-coating, laser remelting and laser forging, which reduces heat input, especially reduces the heat input of the pile leg matrix, inhibits the thermal deformation of the metal matrix and the growth of microstructure grains in the heat-affected zone, inhibits the growth of coarse columnar crystals, and improves the possibility of on-site repair of large pile legs. In addition, the present invention couples the laser remelting and laser forging processes, and laser forges the high-temperature remelted metal layer during the laser remelting process, which can promote dynamic recovery and dynamic recrystallization of the high-temperature metal layer, effectively eliminate residual tensile stress, and realize internal microstructure regulation, refine grains, and reduce irregular pore defects. The elimination of residual tensile stress helps to inhibit stress corrosion of the repair layer. Microstructure refinement helps to improve the wear resistance of the repair layer, and the reduction of pore defects helps to improve the mechanical properties of the repair layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of marine engineering equipment, and in particular to an on-site in-situ remanufacturing method and device for large pile legs of marine engineering equipment. Background Art

[0002] Marine engineering equipment is an important support for the development and utilization of marine resources, such as offshore wind power installation platforms, offshore cranes, and offshore oil and gas drilling platforms. Pile legs are important components of marine engineering equipment, ensuring the stability of the construction process and installation accuracy. However, pile legs that have been working in the marine environment for a long time will inevitably be damaged due to corrosion, wear, etc. The damage to the pile legs affects the stability and safety of the equipment and may cause safety accidents. Therefore, effective measures must be taken to replace or repair the damaged pile legs.

[0003] Remanufacturing methods are used to restore the original size and function of parts, which can greatly reduce costs and save raw materials. The size of the pile legs of marine engineering equipment is generally huge, and the economic significance of restoring their original size by remanufacturing methods is more significant. However, research on pile leg repair, especially methods and equipment for on-site repair, has not been studied and manufactured. Summary of the invention

[0004] The purpose of the present invention is to solve the above-mentioned problems and provide a method and device for on-site in-situ remanufacturing of large pile legs of marine engineering equipment.

[0005] The purpose of the present invention can be achieved by adopting the following technical solutions:

[0006] A method for in-situ remanufacturing of large pile legs of marine engineering equipment comprises the following steps:

[0007] S1: After the pile legs are lifted or lowered to a fixed position, a pile-circling moving system is arranged around the pile legs, including a circular guide rail, a trolley and a manipulator;

[0008] S2: Detect the external dimensions of the pile legs, locate the position and range of damage to the pile legs, and use a flaw detector to detect the length and depth of the cracks in the damaged position of the pile legs;

[0009] S3: Subtract material from the metal matrix at the damaged location to eliminate internal cracks and polish the damaged area to a regular shape;

[0010] S4: Clean the damaged area after material reduction to remove the residue, detect the dimensions of the pile leg, and calculate the amount of damage;

[0011] S5: Use thermal spraying to spray metal coating on the damaged area. The metal coating must completely cover the damaged area of ​​the pile leg. The thickness of the metal coating sprayed once shall not exceed the laser remelting depth under the premise of being close to the maximum damage amount.

[0012] S6: laser remelting the metal coating in the damaged area of ​​the pile leg, and laser forging the high-temperature solidified metal layer during the laser remelting process. The laser remelting and laser forging are performed simultaneously;

[0013] S7: Use a flaw detector to detect whether there are defects in the metal layer after laser remelting. If no defects are found, proceed to the next repair step; if defects are found, repeat step S6 and perform laser remelting again in the defective area, and repeat the above steps until no defects are detected;

[0014] S8: Detect the external dimensions of the damaged area of ​​the pile leg after laser remelting and laser forging, and calculate the repair increment of the damaged area of ​​the pile leg. If the repair increment of the damaged area of ​​the pile leg is a positive value, proceed directly to the next repair step; if the repair increment of the damaged area of ​​the pile leg is a negative value, continue to repeat steps S5, S6, and S7 to detect the external dimensions of the damaged area of ​​the pile leg until the repair increment of the damaged area of ​​the pile leg becomes a positive value;

[0015] S9: Remove the excess part of the repair layer in the damaged area of ​​the pile leg by reducing material to restore the original design size of the pile leg.

[0016] As a preferred solution, the specific content of step S3 is:

[0017] According to the scope and depth of the pile leg damage area, the manipulator is controlled to move to perform subtractive processing on the damaged position of the pile leg; then the damaged position is polished regularly;

[0018] As a preferred solution, the specific content of step S4 is:

[0019] According to the scope of the damaged area, the robot is controlled to move, so that the robot drives the high-pressure water gun to move and remove the residual materials in the grinding area; then, the external dimensions of the damaged area of ​​the pile leg after subtractive processing are detected and the amount of damage is calculated.

[0020] As a preferred solution, the specific content of step S5 is:

[0021] Fix the spray gun to the robot arm, control the robot arm to move, spray the metal coating on the damaged area and make the metal coating completely cover and exceed the damaged area; control the robot arm to drive the spray gun to spray back and forth multiple times, so that the metal coating reaches the set thickness;

[0022] As a preferred solution, the specific content of step S6 is:

[0023] Finite element simulation is used to calculate the temperature change of the laser remelting layer under ambient temperature, and the positions of the two laser beams are adjusted to the set distance; the laser remelting and laser forging laser heads are coupled and fixed together with the manipulator; the manipulator is controlled to move, so that the continuous laser laser head and the pulse laser laser head move synchronously to complete the laser remelting and laser forging;

[0024] As a preferred solution, the specific content of step S9 is:

[0025] S91: Fix the grinding machine on the manipulator, and control the manipulator to drive the grinding machine to move, so as to remove the excess part of the repair layer;

[0026] S92: Detect the external dimensions of the damaged area of ​​the pile leg after repair, and calculate the repair increment of the damaged position; if the repair increment is zero, the repair is completed; if the repair increment is a positive value, repeat step S91 until the repair increment becomes zero.

[0027] A device for on-site in-situ remanufacturing method of large pile legs of marine engineering equipment, comprising a pile leg moving system, a manipulator, a laser three-dimensional scanning detection system, a material reduction system, an X-ray flaw detector, a cleaning system, a spray control system, a laser remelting system and a laser forging system; the pile leg moving system controls the pile moving state of the manipulator; the manipulator drives the laser three-dimensional scanning detection system, the material reduction system, the X-ray flaw detector, the cleaning system, the spray control system, the laser remelting system and the laser forging system System Movement ;

[0028] The laser three-dimensional scanning detection system is used to detect the external dimensions of the pile legs;

[0029] The subtractive system is used to remove the matrix of the damaged part of the pile leg and the excess part of the repair layer;

[0030] The X-ray flaw detector is used to detect internal defects of the pile leg matrix and the laser remelting layer;

[0031] The cleaning system is used to clean the pile leg matrix;

[0032] The spray control system is used to spray the metal coating on the damaged area of ​​the pile leg;

[0033] The laser remelting and laser forging system is used for laser remelting and laser forging of metal coating.

[0034] As a preferred solution, the leg movement system comprises a driving device, a guide rail and a trolley installed on the guide rail, and the driving device drives the trolley to move on the guide rail.

[0035] As a preferred solution, the spray control system adopts one of a supersonic arc spray system, a flame spray system and a plasma spray system.

[0036] As a preferred solution, the laser remelting and laser forging system includes a continuous laser, a continuous laser head, a high-energy pulse laser and a pulse laser head; the continuous laser head is connected to the continuous laser optical fiber, and the pulse laser head is connected to the high-energy pulse laser optical fiber.

[0037] The implementation of the present invention has the following beneficial effects:

[0038] 1. The present invention adopts the methods of thermal spraying pre-coating, laser remelting and laser forging, which reduces the heat input, especially reduces the heat input of the pile leg matrix, inhibits the thermal deformation of the metal matrix and the growth of microstructure grains in the heat-affected zone, inhibits the growth of coarse columnar crystals, and improves the possibility of on-site repair of large pile legs.

[0039] 2. The present invention uses a thermal spraying method to deposit the repair material onto the damaged area, and then uses a laser remelting method to remelt the thermal spray coating to achieve repair, which not only improves material utilization, but also eliminates pores and improves the bonding strength of the repair layer.

[0040] 3. The present invention couples the laser remelting and laser forging processes. During the laser remelting process, the high-temperature remelted metal layer is laser forged, which can promote the dynamic recovery and dynamic recrystallization of the high-temperature metal layer, effectively eliminate the residual tensile stress, and realize the internal microstructure regulation, refine the grains, and reduce irregular pore defects. The elimination of residual tensile stress helps to inhibit stress corrosion of the repair layer. Microstructure refinement helps to improve the wear resistance of the repair layer. The reduction of irregular pore defects helps to improve the mechanical properties of the repair layer.

[0041] 4. The present invention utilizes laser remelting and laser forging processes to achieve multiple remelting and forging of the metal layer, eliminate internal defects such as pores and cracks, and achieve multiple regulation of the microstructure of the metal layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0043] Figure 1 It is a flowchart of the on-site in-situ remanufacturing method of large pile legs of marine engineering equipment of the present invention.

[0044] Figure 2 It is a structural schematic diagram of an on-site in-situ remanufacturing device for large pile legs of marine engineering equipment according to the present invention.

[0045] Figure 3 It is a schematic diagram of thermal spraying processing of an on-site in-situ remanufacturing device for large pile legs of marine engineering equipment according to the present invention.

[0046] Figure 4 It is a processing schematic diagram of laser remelting and laser forging of an on-site in-situ remanufacturing device for large pile legs of marine engineering equipment of the present invention.

[0047] Figure 5 It is a comparison diagram of the position before damage and the position after laser remelting and laser forging in the method for calculating the damage amount of the on-site in-situ remanufacturing method of a large pile leg of marine engineering equipment of the present invention. DETAILED DESCRIPTION

[0048] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] Example

[0050] Reference Figure 1 and Figure 2 This embodiment relates to an on-site in-situ remanufacturing method for large pile legs of marine engineering equipment, comprising the following steps:

[0051] S1: After the pile leg 18 is lifted or lowered to a fixed position, a pile leg movement system is arranged around the pile leg 18, wherein the pile leg movement system comprises a driving device, a guide rail 23 and a trolley 22 mounted on the guide rail, and the driving device drives the trolley 22 to move on the guide rail 23.

[0052] S2: Detect the external dimensions of the pile leg 18 around the pile leg 18, locate the position and range of damage on the pile leg 18, and use a flaw detector to detect the length and depth of the cracks in the located damaged position of the pile leg 18;

[0053] S3: Subtract material from the metal matrix at the damaged position to eliminate internal cracks and grind the damaged area into a regular shape; specifically, according to the range and depth of the damaged area of ​​the pile leg 18, control the manipulator 21 to move to perform subtractive processing on the damaged position of the pile leg 18; and then grind the damaged position into a regular shape;

[0054] S4: Clean the damaged area after material reduction to remove residues, detect the external dimensions of the pile leg 18, and calculate the amount of damage; specifically, according to the scope of the damaged area, control the movement of the manipulator 21 so that the manipulator 21 drives the high-pressure water gun 7 to move and remove the residual material in the grinding area; then, detect the external dimensions of the damaged area of ​​the pile leg 18 after material reduction processing and calculate the amount of damage.

[0055] S5: Spraying a metal coating on the damaged area by a thermal spraying method, the metal coating must completely cover the damaged range of the pile leg 18, and the thickness of the metal coating sprayed once does not exceed the laser remelting depth under the premise of being close to the maximum damage amount; specifically, fixing the spray gun 10 to the manipulator 21, controlling the manipulator 21 to move, spraying the metal coating on the damaged area and making the metal coating completely cover and exceed the damaged area; controlling the manipulator to drive the spray gun to spray back and forth multiple times, so that the metal coating reaches a set thickness;

[0056] S6: laser remelting the metal coating in the damaged area of ​​the pile leg 18, and laser forging the high-temperature solidified metal layer during the laser remelting process, and laser remelting and laser forging are performed simultaneously; specifically, using finite element simulation to calculate the temperature change of the laser remelting layer under ambient temperature, the positions of the two laser beams are adjusted to a set distance; the laser remelting (continuous laser laser head) and the laser forging laser head (high-energy pulse laser laser head) are coupled and fixed together with the manipulator 21; the manipulator 21 is controlled to move, and the continuous laser laser head 14 and the pulse laser laser head 16 are moved to complete the laser remelting and laser forging;

[0057] S7: Use the flaw detector 3 to detect whether there are defects in the metal layer after laser remelting. If no defects are found, proceed to the next repair step; if defects are found, repeat step S6, perform laser remelting and laser forging again in the defective area, and repeat the above steps until no defects are detected;

[0058] S8: Detect the external dimensions of the damaged area of ​​the pile leg 18 after laser remelting and laser forging, and calculate the repair increment of the damaged area of ​​the pile leg 18. If the repair increment of the damaged area of ​​the pile leg 18 is a positive value, directly proceed to the next repair step; if the repair increment of the damaged area of ​​the pile leg 18 is a negative value, continue to repeat steps S5, S6, and S7 to detect the external dimensions of the damaged area of ​​the pile leg 18 until the repair increment of the damaged area of ​​the pile leg 18 becomes a positive value;

[0059] S9: Removing the excess portion of the repair layer in the damaged area of ​​the pile leg 18 by material reduction to restore the original design size of the pile leg 18. This step includes the following steps:

[0060] S91: Fix the grinding machine on the manipulator 21, and control the manipulator 21 to drive the grinding machine to move, so as to remove the excess part of the repair layer;

[0061] S92: Detect the external dimensions of the damaged area of ​​the pile leg 18 after repair, and calculate the repair increment of the damaged position; if the repair increment is zero, the repair is completed; if the repair increment is a positive value, repeat step S91 until the repair increment becomes zero.

[0062] The present embodiment also provides a device for the on-site in-situ remanufacturing method of the above-mentioned large pile legs 18 of marine engineering equipment, including a pile leg movement system, a manipulator 21, a laser three-dimensional scanning detection system 2, a material reduction system 6, an X-ray flaw detector 3, a cleaning system, a spray control system 12, a laser remelting system and a laser forging system; the pile leg movement system controls the pile movement state of the manipulator 21; the laser three-dimensional scanning detection system 2, the material reduction system 6, the X-ray flaw detector 3, the cleaning system, the spray control system 12, the laser remelting system and the laser forging system are arranged on the manipulator 21 and move by the drive of the manipulator; the cleaning system includes a high-pressure water gun 7 and a sealed container 8 for supplying industrial alcohol to the high-pressure water gun.

[0063] The laser three-dimensional scanning detection system is used to detect the external dimensions of the pile leg 18;

[0064] The subtractive system is used to remove the matrix of the damaged part of the pile leg 18 and the excess part of the repair layer;

[0065] The X-ray flaw detector is used to detect internal defects of the pile leg 18 matrix and the laser remelting layer;

[0066] The cleaning system is used to clean the base of the pile leg 18;

[0067] The spray control system is used to spray the metal coating on the damaged area of ​​the pile leg 18;

[0068] The laser remelting and laser forging system is used for laser remelting and laser forging of metal coating.

[0069] The leg-circling movement system comprises a driving device, a guide rail and a trolley 22 mounted on the guide rail. The driving device drives the trolley 22 to move on the guide rail.

[0070] The spray control system adopts one of a supersonic arc spray system, a flame spray system and a plasma spray system.

[0071] The laser remelting and laser forging system comprises a continuous laser, a continuous laser head, a high-energy pulse laser and a pulse laser head; the continuous laser head is connected to the continuous laser optical fiber, and the pulse laser head is connected to the high-energy pulse laser optical fiber.

[0072] The following example illustrates the above method, which is applied to the repair of the E690 steel pile leg of the offshore wind power installation platform. Figures 1 to 4, the method comprises the following steps:

[0073] Step S1: After the offshore wind power installation platform is lifted to a specific position and fixed, a circular guide rail, a trolley 22 and a manipulator 21 are arranged around the pile legs 18;

[0074] Step S2: using a laser three-dimensional scanner to detect the external dimensions of the pile leg 18 around the pile leg 18, importing the data into a computer, analyzing and locating the position and range of damage in the pile leg 18, using an X-ray flaw detector 3 to detect crack defects in the damaged position of the pile leg 18, transmitting the data to a computer, and analyzing the length and depth of the crack; specifically, fixing the laser three-dimensional scanner detector to the manipulator 21, editing instructions through a teach pendant, so that the detector detects the external dimensions of the pile leg 18 around the pile leg 18; then transmitting the data scanned by the detector to the computer, analyzing the data, and determining the damaged position of the pile leg 18; then fixing the X-ray flaw detector to the manipulator 21, editing instructions through a teach pendant, and using the flaw detector detector to detect cracks at the damaged position; finally transmitting the flaw detector detector data to the computer, analyzing the data, and determining the length and depth of the crack;

[0075] Step S3: grinding the E690 steel pile leg matrix at the damaged position by using a grinding wheel machine to eliminate internal cracks and grind the damaged area into a regular pattern; specifically, fixing the grinding wheel machine to the manipulator 21, and editing the movement instructions of the manipulator 21 through the teaching pendant; then grinding the damaged position of the pile leg 18, and the grinding position and depth are determined according to the data detected by the laser three-dimensional scanner and the X-ray flaw detector; finally, further grinding the damaged position into a regular pattern;

[0076] Step S4: Use the high-pressure water gun 7 to spray industrial alcohol to clean the damaged area of ​​the E690 steel substrate after grinding to remove residues, use the laser three-dimensional scanner to detect the size of the pile leg 18, calculate the damage amount, and provide a reference for the thickness of the metal coating sprayed in the next step; specifically, fix the laser three-dimensional scanner detector to the manipulator 21, edit the instructions, detect the size of the damaged area of ​​the pile leg 18 after grinding, and calculate the damage amount; then fix the high-pressure water gun 7 to the manipulator 21, add industrial alcohol to the container; finally, edit the movement instructions of the manipulator 21 through the teaching pendant to clean the grinding area;

[0077] For cylindrical pile legs 18, Figure 5 As shown, the calculation method of the damage amount is as follows: establish a cylindrical coordinate system, find the design size of the undamaged pile leg 18 through the design drawings, and determine the radius of the surface point of the pile leg 18. Since the pile leg 18 is cylindrical, the original radial length r of any point i at the damage position is 1 (i,θ) is a fixed value r, r is the designed outer radius of the pile leg 18, and the radial coordinate after the laser 3D scanner detector detects the damage at point i is r2 (i, θ), then the damage amount is defined as Δr = rr 2 (i, θ).

[0078] Step S5: Use supersonic arc spraying to spray a metal coating on the damaged area. The metal coating must completely cover the damaged range of the pile leg 18. The thickness of the single-sprayed metal coating does not exceed the laser remelting depth under the premise of being close to the maximum damage amount. If the thickness of the thermal sprayed metal coating exceeds the laser remelting thickness, the porosity of the repair layer will increase and the bonding strength will decrease. Specifically, first prepare a special metal wire for E690 steel pile leg repair; then fix the thermal spray gun to the manipulator 21, with the gun perpendicular to the pile leg 18, and teach The device edits the movement instructions of the robot 21; finally, a supersonic arc spraying gun is used to spray the metal coating on the damaged area so that the metal coating completely covers the damaged area and exceeds the damaged area by about 10mm. After multiple reciprocating spraying, the metal coating reaches a certain thickness. The thickness of the single-sprayed metal coating is as close as possible to the maximum value of the damage amount and at the same time is less than the laser remelting depth; the metal spraying parameters can be preferably: current 500-600A, voltage: 50-65V, spraying distance 100-200mm, spraying angle 15-90°.

[0079] Step S6: Use a continuous laser to generate high-energy continuous laser to laser remelt the metal coating sprayed in the damaged area of ​​the pile leg 18. During the laser remelting process, the high-temperature remelted metal layer is laser forged. Laser remelting and laser forging are performed simultaneously. Specifically, the temperature of the laser remelted metal layer determines the evolution mechanism of the microstructure during laser forging. The laser forging temperature must be above the recrystallization temperature. The recrystallization temperature can be found in the manual. The temperature change of the remelted metal coating at ambient temperature can be calculated using finite element simulation. According to the recrystallization temperature and the finite element simulation results, the distance between the continuous laser beam and the pulsed laser beam is adjusted to a suitable position, specifically 2-5mm. The laser remelting and laser forging laser heads are coupled and fixed and then bound to the manipulator 21. Then, the teaching pendant is used to edit instructions to start the continuous laser and the pulsed laser synchronously and move the laser head to complete the laser remelting and laser forging.

[0080] The process parameter range of laser remelting is: power: 2000-3000W, rate: 5-20mm / s, and the process parameter range of laser forging is: pulse energy 6-10J, spot size 2-4mm, frequency 5-20Hz.

[0081] Step S7: Use an X-ray flaw detector to detect the metal layer after laser remelting and laser forging, and transfer the data to the computer to analyze whether there are defects. If no defects are found, proceed to the next repair step; if defects are found, repeat step S6, perform laser remelting and laser forging again in the defective area, re-use the X-ray flaw detector for detection, and repeat the above steps until no defects are detected; since laser remelting may also produce defects such as unfused and cracks, it is necessary to detect the metal coating after remelting. The specific step S7 includes the following steps:

[0082] S7-1 fixes the X-ray flaw detector to the manipulator 21;

[0083] S7-2 uses the teach pendant to edit instructions and detect defects in metal coatings after laser remelting and laser forging;

[0084] S7-3 imports the flaw detection data into the computer and analyzes the flaw detection data. If there is no defect, proceed to the next repair step; if there is a defect, repeat step S6 to perform laser remelting and laser forging again;

[0085] S7-4 repeats steps S7-2 and S7-3. If no defect is found, proceed to the next repair step; if a defect is found, repeat step S6 until the defect is completely eliminated;

[0086] Step S8: Use a laser three-dimensional scanner to detect the external dimensions of the damaged repair area of ​​the pile leg 18 after laser remelting and laser forging, and calculate the repair increment of the damaged area of ​​the pile leg 18. If the repair increment of the damaged area of ​​the pile leg 18 is all positive, proceed directly to the next repair step; if the repair increment of the damaged area of ​​the pile leg 18 is negative, continue to repeat steps S5, S6, and S7 to detect the external dimensions of the damaged area of ​​the pile leg 18, and repeat the above steps until the repair increment of the damaged area of ​​the pile leg 18 is all positive; specifically, use a laser three-dimensional scanning measuring instrument to detect the external dimensions of the damaged area of ​​the pile leg 18 after repair, transfer the data to a computer, and give the repair increment of the repair area; if the repair increment of the damaged position is all positive, proceed directly to the next repair step; if the repair increment of the damaged position is negative, repeat steps S5, S6, and S7 to detect the external dimensions of the damaged area of ​​the pile leg 18 again, until the repair increment of the damaged position is all positive;

[0087] The calculation method of the repair increment of the damaged area of ​​the cylindrical E690 steel pile leg 18 after laser remelting and laser forging is similar to the calculation method of the damage amount before repair. Specifically, a cylindrical coordinate system is established, and the original radial coordinate of a point i at the damage position is given as r using the design dimensions of the undamaged pile leg 18, where r is the outer radius of the pile leg 18, and the radial coordinate detected after repair is R 2 (i,θ), then the repair increment is defined as ΔR(i)=R2 (i,θ)-r.

[0088] Step S9: Remove the excess part of the repair layer in the damaged area of ​​the pile leg 18 by grinding with a grinding machine, reduce the repair increment to zero, and restore the original design size of the pile leg 18. Specifically, the steps include:

[0089] S9-1 fix the manipulator 21 and the grinding wheel machine, and use the grinding wheel machine to remove the excess part of the repair layer according to the current repair margin editing instruction of the repair damaged area;

[0090] S9-2 uses a laser three-dimensional scanner to detect the external dimensions of the damaged area of ​​the pile leg 18 after repair, and calculates the repair increment of the damaged position. If the repair increment is zero, the repair is completed; if the repair increment is a positive value, repeat step S9-1 until the repair increment becomes zero.

[0091] A device is provided for the above-mentioned method for repairing the E690 steel pile leg of an offshore wind power installation platform, such as Figures 2 to 4 As shown, it includes a laser three-dimensional scanner detector 1, a laser three-dimensional scanning detection system 2, an X-ray flaw detector 3, an X-ray flaw detection system 4, a grinding machine 5, a subtractive system 6, a high-pressure water gun 7, a sealed container 8, a high-pressure injection system 9, a spray gun 10, a wire feeding system 11, a spray control system 12, a computer 13, a continuous laser laser head 14, a continuous laser 15, a high-energy pulse laser laser head 16, a high-energy pulse laser 17, a pile leg 18, a pile leg positioning hole 19, a teaching pendant 20, a manipulator 21, a trolley 22, a guide rail 23, an atomizing air pipe 24, spray droplets 25, a thermal spray metal coating 26, a wire feeding roller 27, a thermal spray metal wire 28, a continuous laser 29, a remelting pool 30, a remelting metal layer 31, a pulse laser energy 32, and a laser forging coating area 33.

[0092] The trolley 22 is placed on the guide rail 23, and is used to drive the manipulator 21, the laser three-dimensional scanner detector 1, the grinder 5, the X-ray flaw detector 3, the high-pressure water gun 7, the spray gun 10, the continuous laser 29 device 15 laser head 14, and the high-energy pulse laser 17 laser head 16 to move around the pile leg 18;

[0093] The manipulator 21 is fixed to the trolley 22, and is mainly used to fix the laser three-dimensional scanner detector 1, the grinding machine 5, the X-ray flaw detector 3, the high-pressure water gun 7, the spray gun 10, the continuous laser 29 device 15 laser head 14, and the high-energy pulse laser 32 device 17 laser head 16;

[0094] The laser three-dimensional scanning detection system 2 is used to detect the external dimensions of the pile leg 18;

[0095] The material reduction system 6 is used to remove the matrix of the damaged part of the pile leg 18 and the excess part of the repair layer;

[0096] The X-ray flaw detection system 4 is used to detect internal defects of the pile leg 18 matrix and the remelting layer;

[0097] The high pressure spray system 9 is used to clean the base of the pile leg 18;

[0098] The thermal spray control system 12 is used to spray a metal coating on the damaged area of ​​the pile leg 18;

[0099] The laser remelting laser and the laser forging laser are used for laser remelting and laser forging of metal coatings; the laser remelting laser includes a continuous laser head 14 and a continuous laser 15 connected to the continuous laser head 14 by an optical fiber. The laser forging laser includes a high-energy pulse laser head 16 and a high-energy pulse laser 17 connected to the high-energy pulse laser head 16 by an optical fiber.

[0100] During operation, the guide rail is arranged around the pile leg 18, the trolley 22 is fixed to the guide rail, and the manipulator 21 is fixed to the trolley 22. The laser three-dimensional scanner detector 1 is fixed to the manipulator 21, and the instruction is edited through the teaching pendant 20, so that it can detect from top to bottom around the pile leg 18, find the damaged area of ​​the pile leg 18, transmit the data to the computer 13, and analyze the data to give the damage range. The X-ray flaw detector detector is fixed to the manipulator 21, and the instruction is edited through the teaching pendant 20 to scan the damaged area of ​​the pile leg 18 and give the location and depth of the defect. The grinder 5 is fixed to the manipulator 21, and the instruction is edited through the teaching pendant 20 to grind the damaged area, remove deep defects, and grind the damaged area into a regular area. The high-pressure water gun 7 is fixed to the manipulator 21, and the instruction is edited through the teaching pendant 20 to spray high-pressure industrial ethanol for cleaning. The high-pressure water gun 7 on the manipulator 21 is replaced with the laser three-dimensional scanner detector 1, and the damaged area is scanned to give the damage range. The computer 13 is used to analyze and give the amount of damage. The laser three-dimensional scanner detector 1 on the manipulator 21 is replaced with a thermal spray gun 10, and the instruction is edited through the teach pendant 20 so that the spray gun 10 can scan through the entire damaged area under the condition of a fixed spraying distance. The number of round trips of the spray gun 10 is designed, and a coating with a thickness of 2-5 mm is sprayed using the thermal spray control system 12. The spray gun 10 on the manipulator 21 is replaced with a connecting device for a laser remelting laser head and a laser forging laser head, and the instruction is edited through the teach pendant 20 so that the laser remelting laser head and the laser forging laser head can scan the entire damaged area. The computer 13 controls the opening of the laser remelting laser and the laser forging laser, and the undamaged area is not remelted. The instruction is edited through the teach pendant 20 to control the real-time closing and opening of the remelting laser and the forging laser. The dual laser beam connecting device on the manipulator 21 is replaced with an X-ray flaw detector 3, and the instruction is edited through the teach pendant 20 to complete the flaw detection of the remelting forging area. If defects are found, secondary remelting forging is performed in the defective area. If no defects are found, the next step of processing is performed. Replace the X-ray flaw detector 3 on the manipulator 21 with a laser three-dimensional scanning detector, scan the laser remelting and laser forging areas, and use the computer 13 to process and give the repair increment. If the repair increment is positive, proceed to the next step. If the repair increment is negative, continue the spraying-remelting-forging-flaw detection scanning-three-dimensional scanning process until the repair increment is positive. Finally, fix the grinder 5 to the manipulator 21, edit the instructions through the teaching pendant 20, remove the redundant repair layer, and reduce the repair increment to zero.

[0101] During operation, the wire feeding roller 27 in the thermal spray wire feeding system 11 starts to rotate, feeding the metal wire into the spray gun 10. The two metal wires come into contact to generate discharge, and the metal wires melt into liquid. Under the action of the atomizing gas in the atomizing tube, the liquid metal is atomized into small molten droplets and sprayed into the area to be repaired of the pile leg 18 to form a metal coating.

[0102] During operation, the continuous laser 29 emitted by the laser remelting laser head melts the thermal sprayed metal coating 26 to form a molten pool, and the molten pool cools to form a dense remelted coating. The pulsed laser of the pulsed laser head laser forges the laser remelted coating, and dynamic recovery and dynamic recrystallization occur in the laser forging area, which reduces the tensile stress and defect size inside the coating, reduces irregular pore defects, refines the grains, and improves the corrosion resistance and wear resistance of the repair layer.

[0103] The above disclosure is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of the present invention. Therefore, equivalent changes made according to the claims of the present invention are still within the scope of the present invention.

Claims

1. A method for in-situ remanufacturing of large pile legs of marine engineering equipment, characterized in that: The following steps are involved: S1: After the pile legs are lifted or lowered to a fixed position, a pile-circling moving system is arranged around the pile legs, including a circular guide rail, a trolley and a manipulator; S2: Detect the external dimensions of the pile legs, locate the position and range of damage to the pile legs, and use a flaw detector to detect the length and depth of the cracks in the damaged position of the pile legs; S3: Subtract material from the metal matrix at the damaged location to eliminate internal cracks and polish the damaged area to a regular shape; S4: Clean the damaged area after material reduction to remove the residue, detect the dimensions of the pile leg, and calculate the amount of damage; S5: Use thermal spraying to spray metal coating on the damaged area. The metal coating must completely cover the damaged area of ​​the pile leg. The thickness of the metal coating sprayed once shall not exceed the laser remelting depth under the premise of being close to the maximum damage amount. S6: laser remelting the metal coating in the damaged area of ​​the pile leg, and laser forging the high-temperature solidified metal layer during the laser remelting process. The laser remelting and laser forging are performed simultaneously; S7: Use a flaw detector to detect whether there are defects in the metal layer after laser remelting; if no defects are found, proceed to the next repair step; if defects are found, repeat step S6, perform laser remelting again in the defective area, and repeat the above steps until no defects are detected; S8: Detect the outer dimensions of the pile leg damaged area after laser remelting and laser forging, and calculate the repair increment of the pile leg damaged area; if the repair increment of the pile leg damaged area is a positive value, directly proceed to the next repair step; if the repair increment of the pile leg damaged area is a negative value, continue to repeat steps S5, S6, and S7 to detect the outer dimensions of the pile leg damaged area until the repair increment of the pile leg damaged area becomes a positive value; S9: Remove the excess part of the repair layer in the damaged area of ​​the pile leg by reducing material to restore the original design size of the pile leg.

2. The method for in-situ remanufacturing of large pile legs of marine engineering equipment according to claim 1, characterized in that: The specific content of step S3 is: According to the scope and depth of the pile leg damage area, the robot is controlled to move to perform subtractive processing on the damaged position of the pile leg; then the damaged position is polished regularly.

3. The method for in-situ remanufacturing of large pile legs of marine engineering equipment according to claim 1, characterized in that: The specific content of step S4 is: According to the scope of the damaged area, the robot is controlled to move, so that the robot drives the high-pressure water gun to move and remove the residual materials in the grinding area; then, the external dimensions of the damaged area of ​​the pile leg after subtractive processing are detected and the amount of damage is calculated.

4. The method for in-situ remanufacturing of large pile legs of marine engineering equipment according to claim 1, characterized in that: The specific content of step S5 is: Fix the spray gun to the robot, control the movement of the robot, spray the metal coating on the damaged area and make the metal coating completely cover and exceed the damaged area; control the robot to drive the spray gun to spray back and forth multiple times, so that the metal coating reaches the set thickness.

5. The method for in-situ remanufacturing of large pile legs of marine engineering equipment according to claim 1, characterized in that: The specific content of step S6 is: Finite element simulation is used to calculate the temperature change of the laser remelting layer under ambient temperature, and the positions of the two laser beams are adjusted to the set distance; the laser remelting and laser forging laser heads are coupled and fixed together with the manipulator; the movement of the manipulator is controlled to allow the continuous laser laser head and the pulsed laser laser head to move synchronously to complete the laser remelting and laser forging.

6. The method for in-situ remanufacturing of large pile legs of marine engineering equipment according to claim 1, characterized in that: The specific content of step S9 is as follows: S91: Fix the grinding machine on the manipulator, and control the manipulator to drive the grinding machine to move, so as to remove the excess part of the repair layer; S92: Detect the external dimensions of the damaged area of ​​the pile leg after repair, and calculate the repair increment of the damaged position; if the repair increment is zero, the repair is completed; if the repair increment is a positive value, repeat step S91 until the repair increment becomes zero.

7. A device for on-site in-situ remanufacturing method of large pile legs of marine engineering equipment according to any one of claims 1 to 6, characterized in that: It includes a leg-circling system, a manipulator, a laser three-dimensional scanning detection system, a material reduction system, an X-ray flaw detector, a cleaning system, a spray control system, a laser remelting system and a laser forging system; the leg-circling system controls the manipulator's movement state around the pile; the manipulator drives the laser three-dimensional scanning detection system, the material reduction system, the X-ray flaw detector, the cleaning system, the spray control system, the laser remelting system and the laser forging system to move; The laser three-dimensional scanning detection system is used to detect the external dimensions of the pile legs; The subtractive system is used to remove the matrix of the damaged part of the pile leg and the excess part of the repair layer; The X-ray flaw detector is used to detect internal defects of the pile leg matrix and the laser remelting layer; The cleaning system is used to clean the pile leg matrix; The spray control system is used to spray the metal coating on the damaged area of ​​the pile leg; The laser remelting and laser forging system is used for laser remelting and laser forging of metal coating.

8. The device for on-site in-situ remanufacturing method of large pile legs of marine engineering equipment according to claim 7, characterized in that: The leg movement system around the pile comprises a driving device, a guide rail and a trolley installed on the guide rail, and the driving device drives the trolley to move on the guide rail.

9. The device for on-site in-situ remanufacturing method of large pile legs of marine engineering equipment according to claim 7, characterized in that: The spray control system adopts one of a supersonic arc spray system, a flame spray system and a plasma spray system.

10. The device for on-site in-situ remanufacturing method of large pile legs of marine engineering equipment according to claim 7, characterized in that: The laser remelting and laser forging system comprises a continuous laser, a continuous laser head, a high-energy pulse laser and a pulse laser head; the continuous laser head is connected to the continuous laser optical fiber, and the pulse laser head is connected to the high-energy pulse laser optical fiber.