A method for preparing flower-shaped dendrite cobalt electromagnetic absorbing material
The preparation of flower-like dendrite cobalt electromagnetic wave absorbing material through room temperature solution synthesis has solved the problem of degradation in the absorption performance of existing magnetic metal materials in the high frequency band, achieved the absorption effect of wide band and low density, and provided a lightweight, Efficient electromagnetic wave absorbing material.
Patent Information
- Application Number
- CN202211464287.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-11-22
AI Technical Summary
The electromagnetic wave absorption performance of existing magnetic metal materials in high-frequency bands is affected by eddy currents, resulting in a decrease in magnetic permeability and cannot meet the absorption requirements of wide bands and low density.
The room-temperature solution synthesis method is used to prepare flower-like dendrite cobalt electromagnetic wave absorbing material. By changing the concentration of the sodium hydroxide solution, the thickness of the material is adjusted to form a three-dimensional layered structure to enhance the electromagnetic wave absorption performance.
It realizes lightweight, efficient and wide-band electromagnetic wave absorption performance, with excellent absorption strength and easy-to-regulate absorption performance.
Smart Images

Figure CN115780820B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electromagnetic wave absorbing materials, and more specifically, particularly relates to a method for preparing a flower-shaped dendrite cobalt electromagnetic wave absorbing material. Background Art
[0002] With the popularization of high-frequency communication technology and electronic equipment, the problem of electromagnetic radiation pollution is becoming increasingly serious. Research on electromagnetic wave absorbing materials has received widespread attention from researchers. Meeting the requirements of "strong absorption, broadband, low density, and thin absorption layer" has become the technical standard for commercial electromagnetic wave absorbing materials.
[0003] Among the many candidate materials for absorbers, magnetic metal materials with dual loss mechanisms have become the focus of attention. Magnetic metal materials can exhibit high magnetic permeability in the high frequency band, so they can be widely used in the field of electromagnetic wave absorption materials. However, the high conductivity of magnetic metal materials will form eddy currents in the high frequency band, causing the magnetic permeability to drop sharply, affecting the electromagnetic wave absorption performance of the material. Among them, the flower-like dendrite nanostructure, as a layered nanostructure, has a main trunk and multi-level branches. This branch morphology has a very high specific surface area, which is conducive to enhancing the material's multiple reflection and scattering losses of electromagnetic waves. At the same time, the dendrite structure fully utilizes the interface effect to enhance the magnetoelectric synergy, thereby increasing the absorption bandwidth and realizing the material's efficient absorption of electromagnetic waves. Based on this, we propose a method for preparing a flower-like dendrite cobalt electromagnetic absorber. Summary of the invention
[0004] The purpose of the present invention is to solve the shortcomings of the prior art and propose a method for preparing a flower-shaped dendrite cobalt electromagnetic absorbing material. The magnetic metal Co material is modified to prepare a flower-shaped dendrite cobalt electromagnetic absorbing material. The material has the characteristics of "lightweight, high efficiency, wide frequency and thin layer", and has good absorption characteristics for high-frequency electromagnetic waves.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A method for preparing a flower-shaped dendrite cobalt electromagnetic wave absorbing material comprises the following steps:
[0007] S1, adding cobalt salt and hexadecyltrimethylammonium bromide into deionized water and stirring, and obtaining solution A after the stirring is completed;
[0008] The cobalt salt is one of cobalt nitrate, cobalt chloride and cobalt sulfate, and the molar mass of the cobalt salt is 1.5-2.5 mmol;
[0009] The molar mass of the hexadecyltrimethylammonium bromide is 5mmol-10mmol;
[0010] S2, adding sodium hydroxide solution into deionized water and stirring, after the stirring is completed, obtaining solution B;
[0011] Wherein, the concentration of the sodium hydroxide solution is 10mol / L-20mol / L;
[0012] S3, adding the solution B to the solution A for mixing and stirring, and obtaining solution C after the stirring is completed;
[0013] S4, adding the hydrazine hydrate solution dropwise into the solution C, while stirring the solution C, and obtaining a precipitate D after the stirring is completed;
[0014] S5. Repeatedly wash and dry the reaction product D to obtain a dendrite cobalt electromagnetic wave absorbing material.
[0015] Preferably, the stirring in steps S1, S2, S3 and S4 is magnetic stirring;
[0016] The stirring time in step S1 is 10-90 minutes;
[0017] The stirring time in step S2 is 10-90 minutes;
[0018] The duration of the stirring treatment in step S3 is 30-120 minutes;
[0019] The stirring time in step S4 is 30-120min.
[0020] Preferably, the magnetic stirring adopts a cuvette magnetic stirrer, and the cuvette magnetic stirrer comprises:
[0021] A magnetic stirring system and a control system, wherein the magnetic stirring system is composed of a magnetic stirring device;
[0022] The magnetic stirring system comprises:
[0023] A cuvette and a magnetic stirring head, wherein the cuvette is located in the stirring area of the magnetic stirring head, a tetrafluoro magnetic stirring bar is arranged in the cuvette, and an N-level coil and an S-level coil are arranged inside the magnetic stirring head.
[0024] Preferably, the control system consists of a control box and a circuit assembly, wherein the control box is provided with an MCU and a driver chip, wherein the circuit assembly is a magnetic stirring control circuit, wherein the MCU is connected to the driver chip through an I / O interface in conjunction with the magnetic stirring control circuit, and the driver chip is connected to the magnetic stirring connector through a cable.
[0025] Preferably, the mass fraction of the hydrazine hydrate solution in step S4 is 50wt%, and the volume of the hydrazine hydrate solution is 2mL-6mL.
[0026] Preferably, the washing in step S5 has the following specific process:
[0027] 1) The solid and liquid of the reaction product D are fully stirred to dissolve as much soluble impurities therein as possible in deionized water;
[0028] 2) centrifuging the mixture of the reaction product D and ionized water to remove the liquid phase;
[0029] 3) Repeat the above steps 1) and 2) at least 3 times.
[0030] Preferably, in step S5, the drying temperature of the drying treatment is 40-60° C., and the drying time is 12-24 hours.
[0031] Preferably, the size of the cuvette is 15 mm, the stirrer in the cuvette is a tetrafluoro magnetic stirrer, and the size of the magnetic stirring head is 12 mm×12 mm×8 mm.
[0032] Technical effects and advantages of the present invention: The present invention provides a method for preparing a flower-shaped dendrite cobalt electromagnetic absorbing material. Compared with the traditional preparation method, the present invention adopts a room temperature solution synthesis method to prepare the flower-shaped dendrite cobalt electromagnetic absorbing material. The preparation method is simple to operate, easy to control, and has a short synthesis cycle.
[0033] Secondly, the cobalt electromagnetic wave absorbing material with a three-dimensional layered flower-like dendrite structure prepared by the present invention is composed of a dendrite-shaped metal cobalt single substance; at the same time, by changing the concentration of the sodium hydroxide solution to adjust the thickness of the dendrite cobalt, the absorption capacity of the prepared material to electromagnetic waves can be changed;
[0034] Furthermore, the flower-shaped dendrite cobalt electromagnetic absorbing material prepared by the present invention has excellent electromagnetic wave absorption performance, and has the characteristics of low filling ratio, thin matching thickness, high absorption intensity, wide absorption frequency band, and easy to adjust the absorption performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a synthesis process diagram of the dendrite cobalt magnetic material obtained in Examples 1-3 of the present invention;
[0036] Figure 2 The XRD spectrum of the dendrite cobalt magnetic material obtained in Example 1-3 of the present invention;
[0037] Figure 3 This is a SEM spectrum of the dendrite cobalt magnetic material obtained in Example 1 of the present invention;
[0038] Figure 4This is a SEM spectrum of the dendrite cobalt magnetic material obtained in Example 2 of the present invention;
[0039] Figure 5 This is a SEM spectrum of the dendrite cobalt magnetic material obtained in Example 3 of the present invention;
[0040] Figure 6 This is a curve diagram showing the change of reflection loss of the dendrite cobalt electromagnetic absorbing material at different thicknesses as a function of frequency obtained in Example 1 of the present invention;
[0041] Figure 7 This is a curve diagram showing the change of reflection loss of the dendrite cobalt electromagnetic absorbing material with frequency at different thicknesses obtained in Example 2 of the present invention;
[0042] Figure 8 This is a curve diagram showing the change of reflection loss of the dendrite cobalt electromagnetic absorbing material with frequency at different thicknesses obtained in Example 3 of the present invention;
[0043] Fig. 9 This is a curve diagram showing the variation of the attenuation constant of the dendrite cobalt electromagnetic absorbing material of Examples 1-3 of the present invention with respect to frequency;
[0044] Fig.10 The impedance matching curve of the dendrite cobalt electromagnetic absorbing material obtained in Examples 1-3 of the present invention varies with frequency. DETAILED DESCRIPTION
[0045] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0046] The present invention provides a method for preparing a flower-shaped dendrite cobalt electromagnetic wave absorbing material, comprising the following steps:
[0047] S1, adding cobalt salt and hexadecyltrimethylammonium bromide into deionized water and stirring, and obtaining solution A after the stirring is completed;
[0048] The cobalt salt is one of cobalt nitrate, cobalt chloride and cobalt sulfate, and the molar mass of the cobalt salt is 1.5-2.5 mmol;
[0049] The molar mass of hexadecyltrimethylammonium bromide is 5mmol-10mmol;
[0050] S2, adding sodium hydroxide solution into deionized water and stirring, after the stirring is completed, obtaining solution B;
[0051] Wherein, the concentration of sodium hydroxide solution is 10mol / L-20mol / L;
[0052] S3, adding solution B to solution A for mixing and stirring, and obtaining solution C after the stirring is completed;
[0053] S4, adding the hydrazine hydrate solution dropwise into solution C, stirring solution C at the same time, and obtaining a precipitate D after the stirring is completed;
[0054] The mass fraction of the hydrazine hydrate solution in step S4 is 50wt%, and the volume of the hydrazine hydrate solution is 2mL-6mL;
[0055] S5, repeatedly washing and drying the reaction product D to obtain a dendrite cobalt electromagnetic wave absorbing material;
[0056] The specific process of washing in step S5 is as follows:
[0057] 1) The solid and liquid of the reaction product D are fully stirred to dissolve as much soluble impurities therein as possible in deionized water;
[0058] 2) centrifuging the mixture of the reaction product D and ionized water to remove the liquid phase;
[0059] 3) Repeat the above steps 1) and 2) at least 3 times.
[0060] Wherein, the stirring in steps S1, S2, S3 and S4 is magnetic stirring;
[0061] The duration of the stirring treatment in step S1 is 10-90 minutes;
[0062] The stirring time in step S2 is 10-90 minutes;
[0063] The duration of the stirring treatment in step S3 is 30-120 minutes;
[0064] The duration of the stirring treatment in step S4 is 30-120 minutes.
[0065] The magnetic stirring adopts a cuvette magnetic stirrer, which includes:
[0066] Magnetic stirring system and control system. The magnetic stirring system consists of magnetic stirring equipment;
[0067] The magnetic stirring system includes:
[0068] The cuvette and magnetic stirring head are provided, the size of the cuvette is 15 mm, the stirring bar in the cuvette is a polyfluoro magnetic stirring bar, the size of the magnetic stirring head is 12 mm×12 mm×8 mm, the cuvette is located in the stirring area of the magnetic stirring head, the cuvette is provided with a polyfluoro magnetic stirring bar, and the magnetic stirring head is provided with an N-level coil and an S-level coil; the control system is composed of a control box and a circuit component, the control box is provided with an MCU and a driver chip, the circuit component is a magnetic stirring control circuit, the MCU is connected to the driver chip through an I / O interface in conjunction with the magnetic stirring control circuit, and the driver chip is connected to the magnetic stirring connector through a cable.
[0069] In order to make the above-mentioned objects, features and advantages of the present invention more clearly understood, the technical solutions of the present invention are further described below in conjunction with embodiments. However, the present invention is not limited to the embodiments listed, and should also include any other known changes within the scope of the rights claimed by the present invention.
[0070] The term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0071] Example 1
[0072] This implementation case shows a method for preparing a flower-shaped dendrite cobalt electromagnetic absorbing material according to the following steps:
[0073] Step 1: Add 1.5 mmol of cobalt nitrate and 5 mmol of hexadecyltrimethylammonium bromide into 12 mL of deionized water and stir magnetically for 10 min to obtain solution A.
[0074] Step 2: Add 0.16 mol of sodium hydroxide to 16 mL of deionized water and stir magnetically for 10 min to obtain solution B.
[0075] Step 3: Add solution B to solution A, and magnetically stir solution A for 30 minutes. After stirring, solution C is obtained.
[0076] Step 4: while adding 2 mL of 50 wt% hydrazine hydrate dropwise into solution C, magnetically stirring solution C for 30 min, after the stirring was completed, a precipitate D was obtained;
[0077] Step 5: After the reaction is completed, the reaction product is taken out and repeatedly washed three times, placed in a vacuum drying oven at 40° C. for 12 hours, and taken out to obtain a dendrite cobalt electromagnetic absorbing material.
[0078] Example 2
[0079] This implementation case shows a method for preparing a flower-shaped dendrite cobalt electromagnetic absorbing material according to the following steps:
[0080] Step 1: Add 2.0 mmol of cobalt chloride and 7.5 mmol of hexadecyltrimethylammonium bromide into 12 mL of deionized water and stir magnetically for 60 min to obtain solution A.
[0081] Step 2: Add 0.24 mol of sodium hydroxide to 16 mL of deionized water and stir magnetically for 60 min to obtain solution B.
[0082] Step 3: Add solution B to solution A, and magnetically stir solution A for 60 minutes. After stirring, solution C is obtained.
[0083] Step 4: 4 mL of 50 wt% hydrazine hydrate was added dropwise to solution C, and solution C was magnetically stirred for 60 min. After the stirring was completed, a precipitate D was obtained;
[0084] Step 5: After the reaction is completed, the reaction product is taken out and repeatedly washed three times, placed in a vacuum drying oven at 50° C. for 18 hours, and taken out to obtain a dendrite cobalt electromagnetic absorbing material.
[0085] Example 3
[0086] This implementation case shows a method for preparing a flower-shaped dendrite cobalt electromagnetic absorbing material according to the following steps:
[0087] Step 1: Add 2.5 mmol of cobalt sulfate and 10 mmol of hexadecyltrimethylammonium bromide into 12 mL of deionized water and stir magnetically for 90 min to obtain solution A.
[0088] Step 2: Add 0.32 mol of sodium hydroxide to 16 mL of deionized water and stir magnetically for 90 min to obtain solution B.
[0089] Step 3: Add solution B to solution A, and magnetically stir solution A for 120 minutes. After stirring, solution C is obtained.
[0090] Step 4: while adding 6 mL of 50 wt% hydrazine hydrate dropwise into solution C, magnetically stirring solution C for 120 min, after the stirring was completed, a precipitate D was obtained;
[0091] Step 5: After the reaction is completed, the reaction product is taken out and repeatedly washed, placed in a vacuum drying oven at 60° C. for 24 hours, and taken out to obtain a dendrite cobalt electromagnetic absorbing material.
[0092] In summary, the dendrite cobalt electromagnetic absorbing materials prepared in Examples 1-3 were tested.
[0093] According to the test results, the following conclusions are drawn:
[0094] The X-ray diffraction (XRD) patterns of the dendrite cobalt electromagnetic absorbing material samples of Examples 1-3 are as follows: Figure 2 shown. Figure 2 It is shown that Examples 1-3 present four peaks at 41.7°, 44.8°, 47.6° and 75.9. These diffraction peaks are consistent with the positions corresponding to the (100), (002), (101) and (110) crystal planes of hexagonal Co (JCPDS No. 050727). This shows that the electromagnetic absorbing material prepared by us is composed of hexagonal cobalt and has no other impurities.
[0095] The scanning electron microscope (SEM) images of the samples of Examples 1-3 are as follows: Figure 3-5 As shown. We successfully prepared a three-dimensional hierarchical flower-like dendrite structure. The prepared flower-like dendrite cobalt is mainly composed of a long trunk and secondary secondary and tertiary branches. The dendrite has a layered assembly, and most of the secondary branches are parallel to each other and appear at an angle of about 60° relative to the central trunk. Similar structures are also found in the secondary and tertiary branches. The roots of the monolithic branched dendrite structure layers are closely attached, and the tips grow in different directions, eventually forming a clustered dendrite flower.
[0096] In order to evaluate the electromagnetic wave absorption performance of dendrite cobalt electromagnetic wave absorbing materials, we can calculate its reflection loss value according to the transmission line theory. 60wt% of single crystal cobalt electromagnetic wave absorbing material and 40wt% of paraffin wax were prepared into concentric rings (outer diameter 7.00mm, inner diameter 3.04mm, thickness 2.00mm), and the electromagnetic wave absorption performance of the sample was measured by vector network analyzer and simulated and calculated. The reflection loss and frequency curve of the sample is shown in the figure below. Figure 6-8 shown.
[0097] from Figure 6 It can be seen that when the matching thickness is 5.5 mm, the best reflection loss of Example 1 at 16.4 GHz is -15.8 dB, the reflection loss intensity in the range of 14.8-17.2 GHz is below -10 dB, and the effective absorption width is 2.4 GHz. Figure 7 It can be seen that when the matching thickness is 3.5 mm, the best reflection loss of Example 2 at 12.5 GHz is -17.0 dB, the reflection loss intensity in the range of 10.1-14.5 GHz is below -10 dB, and the effective absorption bandwidth reaches 4.4 GHz. Figure 8It can be seen that when the matching thickness is 5.5 mm, the best reflection loss of Example 3 at 16.8 GHz is -43.2 dB, the reflection loss intensity in the range of 15.4-18.0 GHz is below -10 dB, and the effective absorption bandwidth is 2.6 GHz. From the above experimental results, it can be seen that Example 3 has excellent electromagnetic wave absorption performance with high absorption intensity, wide absorption bandwidth and low thickness.
[0098] According to the electromagnetic wave absorption theory, the electromagnetic wave absorption performance of the absorbing material is also related to the attenuation constant and impedance matching. The attenuation constant characterizes the composite material's ability to attenuate electromagnetic waves, and the impedance matching affects the composite material's absorption efficiency of incident electromagnetic waves. The impedance matching value of an ideal electromagnetic wave absorbing material is 1, at which point the incident electromagnetic wave can completely enter the material. When the impedance matching value is in the range of 0.8-1.2, it can be considered that the prepared composite material has good impedance matching in the actual application environment.
[0099] Fig. 9 : is the attenuation constant diagram of sample embodiment 1 to embodiment 3. It can be seen that the attenuation constant value of embodiment 3 is the largest, and the maximum value is 550, indicating that embodiment 3 has the strongest attenuation ability for incident electromagnetic waves. Fig.10 The impedance matching of Examples 1 to 3 at a thickness of 3.5 mm is shown. It can be seen that the peak values of the impedance matching of Examples 1 and 2 are greater than 1.2, indicating that they have poor impedance matching. The peak value of the impedance matching of Example 3 is about 0.9, indicating that it has excellent impedance matching, which can allow more electromagnetic waves to enter the interior of the material, thereby effectively attenuating the electromagnetic waves.
[0100] From the test results of the above embodiments, it can be seen that the present invention adopts a room temperature solution synthesis method to prepare a flower-shaped dendrite cobalt electromagnetic absorbing material. The preparation method is simple to operate, easy to control, and has a short synthesis cycle. Sample Example 3 has the best comprehensive absorbing performance. When the thickness is 5.5 mm, the maximum absorption intensity can reach -43.2 dB, and the effective absorption bandwidth reaches 2.6 GHz. Therefore, the prepared dendrite cobalt electromagnetic absorbing material is an ideal lightweight ultra-thin absorbing material.
[0101] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a flower-shaped dendrite cobalt electromagnetic absorbing material, characterized in that: The steps include: S1, adding cobalt salt and hexadecyltrimethylammonium bromide into deionized water and stirring, and obtaining solution A after the stirring is completed; The cobalt salt is one of cobalt nitrate, cobalt chloride and cobalt sulfate, and the molar mass of the cobalt salt is 1.5-2.5 mmol; The molar mass of the hexadecyltrimethylammonium bromide is 5mmol-10mmol; S2, adding sodium hydroxide solution into deionized water and stirring, after the stirring is completed, obtaining solution B; Wherein, the concentration of the sodium hydroxide solution is 10mol / L-20mol / L; S3, adding the solution B to the solution A for mixing and stirring, and obtaining solution C after the stirring is completed; S4, adding the hydrazine hydrate solution dropwise to the solution C, stirring the solution C, and obtaining a precipitate D after the stirring is completed; the mass fraction of the hydrazine hydrate solution in the step S4 is 50wt%, and the volume of the hydrazine hydrate solution is 2mL-6mL; S5, repeatedly washing and drying the reaction product D to obtain a dendrite cobalt electromagnetic wave absorbing material; The specific process of washing in step S5 is as follows: 1) The solid and liquid of the reaction product D are fully stirred to dissolve as much soluble impurities therein as possible in deionized water; 2) centrifuging the mixture of the reaction product D and ionized water to remove the liquid phase; 3) Repeat the above steps 1) and 2) at least 3 times; The drying temperature of the drying treatment is 40-60° C., and the drying time is 12-24 hours.
2. The method for preparing a flower-shaped dendrite cobalt electromagnetic absorbing material according to claim 1, characterized in that: The stirring described in steps S1, S2, S3 and S4 is magnetic stirring; The stirring time in step S1 is 10-90 minutes; The stirring time in step S2 is 10-90 minutes; The duration of the stirring treatment in step S3 is 30-120 minutes; The duration of the stirring treatment in step S4 is 30-120 minutes.
3. The method for preparing a flower-shaped dendrite cobalt electromagnetic absorbing material according to claim 2, characterized in that: The magnetic stirring adopts a cuvette magnetic stirrer, and the cuvette magnetic stirrer comprises: A magnetic stirring system and a control system, wherein the magnetic stirring system is composed of a magnetic stirring device; The magnetic stirring system comprises: A cuvette and a magnetic stirring head, wherein the cuvette is located in the stirring area of the magnetic stirring head, a tetrafluoro magnetic stirring bar is arranged in the cuvette, and an N-level coil and an S-level coil are arranged inside the magnetic stirring head.
4. The method for preparing a flower-shaped dendrite cobalt electromagnetic absorbing material according to claim 3, characterized in that: The control system consists of a control box and a circuit component. The control box is provided with an MCU and a driver chip. The circuit component is a magnetic stirring control circuit. The MCU is connected to the driver chip through an I / O interface in conjunction with the magnetic stirring control circuit. The driver chip is connected to the magnetic stirring connector through a cable.
5. The method for preparing a flower-shaped dendrite cobalt electromagnetic absorbing material according to claim 3, characterized in that: The size of the cuvette is 15 mm, the stirring bar in the cuvette is a tetrafluoro magnetic stirring bar, and the size of the magnetic stirring head is 12 mm×12 mm×8 mm.
Citation Information
Patent Citations
Synthetic method of nanometer materials of cobalt fractal structure
CN103170646A
Preparation method for flower-like cobalt particles
CN105834453A
Preparation method for multi-branched nano-alloy electrocatalyst
CN108526481A
Core-shell structure C@CoNi composite material as well as preparation method and application thereof
CN110666157A
Cobalt particle with multi-stage lamellar structure as well as preparation method and application of cobalt particle
CN111482619A