A submicron spherical alpha-phase alumina and preparation method thereof
By mixing and calcining submicron spherical γ-phase alumina with large-particle size thermally conductive fillers and performing ball milling, the problem of sintering of submicron spherical alumina after calcination is solved, its sphericity and α-phase content are improved, and the thermal conductivity is enhanced.
Patent Information
- Application Number
- CN202211519207.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-30
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-11-30
AI Technical Summary
It is difficult to increase the alpha phase content of submicron spherical alumina and maintain its sphericity at the same time with the existing technology. In particular, signs of sintering tend to appear during the calcination process, which affects the thermal conductivity.
By mixing submicron spherical γ phase alumina with large particle size thermally conductive fillers and then calcining it at high temperature, combined with wet ball milling and sieving drying, a submicron spherical α phase with a sphericity greater than 90% and an α phase content greater than 50% is prepared. aluminum oxide.
The sphericity and alpha phase content of submicron spherical alumina are improved, its thermal conductivity effect in thermal conductive materials is enhanced, sintering is avoided, and the morphological stability of the product is improved.
Smart Images

Figure CN115784277B_ABST
Abstract
Description
Technical field:
[0001] The invention relates to the technical field of inorganic powder preparation, and in particular to submicron spherical alpha-phase alumina and a preparation method thereof. Background technology:
[0002] α-phase submicron (0.1-1μm) spherical alumina has the properties of high thermal conductivity, high hardness, high temperature resistance, corrosion resistance, wear resistance, good fluidity, low oil absorption value, small specific surface area, etc. It is widely used in thermal conductive interface materials, thermal conductive engineering plastics and fillers for aluminum-based copper clad laminates.
[0003] The invention patent with publication number CN106629799A, "A method for synthesizing aluminum oxide powder by combustion", synthesizes submicron spherical aluminum oxide by burning aluminum powder and oxygen. However, the submicron spherical aluminum oxide produced by the method by technicians in the field is not good through XRD test (see attached). Figure 2 ) shows that the α-phase content is relatively low.
[0004] The usual method to increase the α-phase content of alumina, such as industrial alumina powder (γ-Al2O3), is to calcine the alumina at above 1200°C to cause it to undergo a reconstructed crystal transformation. However, submicron spherical alumina is highly active and often shows severe signs of sintering during the calcination process. This is because submicron spherical alumina undergoes a reconstructed crystal transformation during high-temperature calcination, accompanied by the formation of a liquid phase. Submicron particles are prone to agglomeration, resulting in severe signs of sintering after calcination. If it is dispersed by ball milling, its spherical morphology cannot be maintained.
[0005] The invention patent with publication number CN111484050B, "A method for preparing quasi-spherical α-phase nano-alumina", uses industrial alumina as raw material, and prepares quasi-spherical α-phase nano-alumina powder through grinding, adding additives, ultrasound, pre-sintering, calcining and other operations, and the Na2O content in the alumina powder is less than 0.02%, which solves the problem that the existing technology cannot simultaneously achieve nano- and spherical alumina powder. However, it can be seen from the scanning electron microscope image that the alumina obtained has poor sphericity and a drum-like morphology. Summary of the invention:
[0006] The technical problem to be solved by the present invention is to provide a submicron spherical α-phase alumina and a preparation method thereof, adopt a calcination process to increase the α-phase content of the submicron spherical alumina, solve the problem of powder sintering of the submicron spherical alumina after calcination, and maintain the sphericity of the submicron alumina.
[0007] The technical problem to be solved by the present invention is achieved by adopting the following technical solutions:
[0008] One of the purposes of the present invention is to provide a submicron spherical α-phase alumina with a sphericity greater than 90%, an α-phase content greater than 50%, and a D50 particle size of 0.2-0.9 μm.
[0009] The second object of the present invention is to provide a method for preparing submicron spherical α-phase alumina, which is prepared by calcining submicron spherical γ-phase alumina and large-particle thermal conductive filler.
[0010] The specific steps include:
[0011] (1) mixing submicron spherical γ-phase alumina and large-particle thermal conductive filler uniformly;
[0012] (2) placing the uniformly mixed materials into a muffle furnace for high-temperature calcination;
[0013] (3) the product obtained after calcination is wet ball milled;
[0014] (4) Screening and drying the ball-milled material to obtain submicron spherical α-phase alumina.
[0015] The beneficial effects of the present invention are:
[0016] (1) The submicron spherical α-phase alumina obtained by the present invention has a high sphericity and α-phase content, which can improve its thermal conductivity in thermal conductive materials.
[0017] (2) The present invention mixes submicron spherical γ-phase alumina with large-particle thermal conductive filler and calcines them simultaneously. Since the submicron spherical γ-phase alumina has high activity, it is adsorbed on the surface of the large-particle thermal conductive filler, thereby avoiding sintering between the submicron spherical γ-phase alumina particles.
[0018] (3) Compared with calcining submicron spherical γ-phase alumina alone, due to the good thermal conductivity of large-particle thermal conductive fillers, at the same calcination temperature, the α-phase content of the product obtained by mixing it with submicron spherical γ-phase alumina and calcining it is higher. Description of the drawings:
[0019] Figure 1 This is the XRD pattern of commercially available micron-spherical α-phase alumina;
[0020] Figure 2 The XRD pattern of the raw material submicron spherical γ-phase alumina;
[0021] Figure 3 This is the XRD pattern of the submicron spherical α-phase alumina product of Example 1;
[0022] Figure 4 This is the XRD pattern of the submicron spherical α-phase alumina product of Example 2;
[0023] Figure 5This is a SEM image of the submicron spherical α-phase alumina product of Example 3;
[0024] Figure 6 This is the XRD pattern of the submicron spherical α-phase alumina product of Example 3;
[0025] Figure 7 The XRD diagram of the submicron spherical α-phase alumina of the product of comparative example 1;
[0026] Figure 8 The XRD diagram of the submicron spherical α-phase alumina of the product of comparative example 2;
[0027] Fig. 9 This is the SEM image of the submicron spherical α-phase alumina of the product of Control Example 3;
[0028] Fig.10 This is the SEM image of the submicron spherical α-phase alumina of the product of Control Example 4. Specific implementation method:
[0029] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below in conjunction with specific embodiments and diagrams.
[0030] The above-mentioned commercially available micron-spherical α-phase alumina comes from Anhui Yishitong Materials Technology Co., Ltd., with the brand name HJA-800.
[0031] One of the purposes of the present invention is to provide a submicron spherical α-phase alumina with a sphericity greater than 90%, an α-phase content greater than 50%, and a D50 particle size of 0.2-0.9 μm.
[0032] Preferably, the α-phase content of the submicron spherical α-phase alumina is greater than 80%.
[0033] The second object of the present invention is to provide a method for preparing submicron spherical α-phase alumina, which is prepared by calcining submicron spherical γ-phase alumina and large-particle thermal conductive filler.
[0034] The specific steps include:
[0035] (1) mixing submicron spherical γ-phase alumina and large-particle thermal conductive filler uniformly;
[0036] (2) placing the uniformly mixed materials into a muffle furnace for high-temperature calcination;
[0037] (3) the product obtained after calcination is wet ball milled;
[0038] (4) Screening and drying the ball-milled material to obtain submicron spherical α-phase alumina.
[0039] Preferably, the weight ratio of the submicron spherical γ-phase alumina to the large-particle thermal conductive filler is (20-30):(70-80).
[0040] Preferably, the submicron spherical γ-phase alumina has a sphericity greater than 90%, an α-phase content less than 10%, and a D50 particle size of 0.1-1 μm.
[0041] Preferably, the D50 particle size of the large-particle thermal conductive filler is greater than 70 μm, and the shape is spherical or angular, and more preferably spherical.
[0042] The thermal conductivity of the large-particle thermally conductive filler is greater than 20 W / (m·K), and is selected from at least one of aluminum oxide and aluminum nitride. Other thermally conductive fillers can also be selected as long as they can withstand the calcination temperature of the present invention.
[0043] Preferably, the calcination temperature is 1200-1400° C., and the calcination time is 2-10 h.
[0044] Preferably, the wet ball milling is a stirring ball milling, the stirring frequency is 100-200 Hz, the stirring time is 10-60 min, and the solid content of the powder is 10-30%.
[0045] The submicron spherical γ-phase alumina used as a raw material in the following examples and comparative examples is prepared by the method disclosed in patent CN106629799A.
[0046] Example 1
[0047] Take 100g of submicron spherical γ-phase alumina (D50 is 0.8μm, α-phase content is 5%, sphericity is 93.5%) and 400g of spherical alumina (D50 is 90μm, α-phase content is 43.2%) in a homogenizer and mix them evenly. Add the evenly mixed materials to the sagger, and then calcine them at 1300℃ in a muffle furnace for 3h. Take 100g of the calcined material and 400g of deionized water in a three-necked flask, and add 150g of zirconium beads. Turn on stirring, set the stirring frequency to 100Hz, and the stirring time to 60min. After separating the zirconium beads, pass through a 325-mesh sieve, and the sieve-surface material obtained is spherical alumina (D50 is 90μm, α-phase content is 68%); then pass through a sieve with a mesh of 20μm, dry the sieve-surface material obtained, and obtain submicron spherical α-phase alumina. The D50 of the submicron spherical α-phase alumina was measured to be 0.81 μm, the α-phase content was 51.9%, and the sphericity was 93.1%.
[0048] Example 2
[0049] Take 100g of submicron spherical γ-phase alumina (D50 is 0.8μm, α-phase content is 5%, sphericity is 93.5%) and 400g of spherical alumina (D50 is 90μm, α-phase content is 43.2%) in a homogenizer and mix them evenly. Add the evenly mixed materials to the sagger, and then calcine them at 1350℃ in a muffle furnace for 3h. Take 100g of the calcined material and 400g of deionized water in a three-necked flask, and add 150g of zirconium beads. Turn on stirring, set the stirring frequency to 200Hz, and the stirring time to 10min. After separating the zirconium beads, pass through a 325-mesh sieve, and the sieve-surface material obtained is spherical alumina (D50 is 90μm, α-phase content is 72%); then pass through a sieve with a mesh of 20μm, dry the sieve-surface material obtained, and obtain submicron spherical α-phase alumina. The D50 of the submicron spherical α-phase alumina was measured to be 0.84 μm, the α-phase content was 68.7%, and the sphericity was 92.9%.
[0050] Example 3
[0051] Take 100g of submicron spherical γ-phase alumina (D50 is 0.8μm, α-phase content is 5%, and sphericity is 93.5%) and 400g of spherical alumina (D50 is 90μm, α-phase content is 43.2%) in a homogenizer and mix them evenly. Add the evenly mixed materials to the sagger, and then calcine them at 1400℃ in a muffle furnace for 3h. Take 100g of the calcined material and 400g of deionized water in a three-necked flask, and add 150g of zirconium beads. Turn on stirring, set the stirring frequency to 150Hz, and the stirring time to 30min. After separating the zirconium beads, pass through a 325-mesh sieve, and the sieve-surface material obtained is spherical alumina (D50 is 90μm, α-phase content is 91%); then pass through a sieve with a mesh of 20μm, dry the sieve-surface material obtained, and obtain submicron spherical α-phase alumina. The D50 of the submicron spherical α-phase alumina was measured to be 0.83 μm, the α-phase content was 88.3%, and the sphericity was 93.8%.
[0052] Example 4
[0053] The only difference from Example 1 is that submicron spherical γ-phase alumina (D50 of 0.2 μm, α-phase content of 5%, sphericity of 94.1%) is used to prepare submicron spherical α-phase alumina. The D50 of the submicron spherical α-phase alumina is measured to be 0.22 μm, the α-phase content is 51.5%, and the sphericity is 93.7%.
[0054] Example 5
[0055] The only difference from Example 1 is that spherical alumina (D50 is 70 μm, α phase content is 41.9%) is used to prepare submicron spherical α phase alumina. The D50 of the submicron spherical α phase alumina is measured to be 0.78 μm, the α phase content is 51.0%, and the sphericity is 92.8%.
[0056] Example 6
[0057] The only difference from Example 1 is that spherical alumina (D50 is 120 μm, α phase content is 48.5%) is used to prepare submicron spherical α phase alumina. The D50 of the submicron spherical α phase alumina is measured to be 0.81 μm, the α phase content is 53.1%, and the sphericity is 93.7%.
[0058] Example 7
[0059] The only difference from Example 1 is that angular alumina (D50 is 90 μm, α phase content is 43.2%) is used to prepare submicron spherical α phase alumina. The D50 of the submicron spherical α phase alumina is measured to be 0.81 μm, the α phase content is 50.8%, and the sphericity is 92.5%.
[0060] Example 8
[0061] The only difference from Example 1 is that 150 g of submicron spherical γ-phase alumina (D50 of 0.8 μm, α-phase content of 5%, sphericity of 93.5%) and 350 g of spherical alumina (D50 of 90 μm, α-phase content of 43.2%) are used to prepare submicron spherical α-phase alumina. The D50 of the submicron spherical α-phase alumina is measured to be 0.79 μm, the α-phase content is 52.5%, and the sphericity is 94.2%.
[0062] Example 9
[0063] The only difference from Example 1 is that spherical aluminum nitride (D50 is 90 μm) is used to prepare submicron spherical α-phase aluminum oxide. The D50 of the submicron spherical α-phase aluminum oxide is measured to be 0.81 μm, the α-phase content is 52.3%, and the sphericity is 93.7%.
[0064] Comparative Example 1
[0065] The only difference from Example 1 is that no spherical alumina is added. The D50 of the submicron spherical α-phase alumina is measured to be 0.85 μm, the α-phase content is 35.2%, and the sphericity is 93.5%.
[0066] Comparative Example 2
[0067] The only difference from Example 1 is that no spherical alumina is added and the calcination temperature is 1350° C. The D50 of the submicron spherical α-phase alumina is measured to be 0.82 μm, the α-phase content is 45.4%, and the sphericity is 93.8%.
[0068] Comparative Example 3
[0069] The only difference from Control Example 1 is that no spherical alumina is added and the calcination temperature is 1400° C. The D50 of the submicron spherical α-phase alumina is measured to be 0.84 μm, the α-phase content is 72%, and the sphericity is 32.2%.
[0070] Comparative Example 4
[0071] The only difference from Example 1 is that 200 g of submicron spherical γ-phase alumina (D50 of 0.8 μm, α-phase content of 5%, sphericity of 93.5%) and 300 g of spherical alumina (D50 of 90 μm, α-phase content of 43.2%) are used to prepare submicron spherical α-phase alumina. The D50 of the submicron spherical α-phase alumina is measured to be 0.88 μm, the α-phase content is 51.4%, and the sphericity is 60.5%.
[0072] Application Example 1-14
[0073] The submicron spherical α-phase alumina obtained in Examples 1-9 and Comparative Examples 1-4, and the raw material submicron spherical γ-phase alumina were added to the vinyl silicone oil system in the same proportion, with a silicone oil viscosity of 450 mPa·s and a filling amount of 45%. The thermal conductivity was tested using ISO22007-2-2008 standard, see Table 1.
[0074] Table 1
[0075]
[0076]
[0077] The α-phase contents of the submicron spherical alumina prepared in Example 2 and Control Example 3 are 68.7% and 72%, respectively, and the α-phase contents are not much different. According to long-term practice, when the α-phase contents are similar, the thermal conductivity of alumina with low sphericity will be better. The thermal conductivity of the submicron spherical alumina prepared in Control Example 3 is higher than that in Example 2. This is due to the non-spherical morphology of the spherical alumina in Control Example 3. However, the viscosity of the spherical alumina prepared in Control Example 3 is significantly increased when added to silicone oil in the same proportion as that in Example 2, which will reduce the maximum amount of thermally conductive filler added. The viscosity data is shown in Table 2.
[0078] Table 2
[0079] Viscosity mPa·s Application Example 2 Submicron spherical α-phase alumina prepared in Example 1 118000 Application Example 13 Submicron spherical α-phase alumina prepared in comparative example 3 176000
[0080] The mixtures of submicron spherical alumina and large-particle thermal conductive fillers before and after calcination in Examples 1 and 9 were added to the vinyl silicone oil system in the same proportions. The silicone oil viscosity was 450 mPa·s and the filling amount was 45%. The thermal conductivity effect was tested using the ISO22007-2-2008 standard, as shown in Table 3.
[0081] Table 3
[0082]
[0083] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A submicron spherical α-phase alumina, characterized in that: The submicron spherical α-phase alumina has a sphericity greater than 90%, an α-phase content greater than 50%, and a D50 particle size of 0.2-0.9 μm; The submicron spherical α-phase alumina is prepared by calcining submicron spherical γ-phase alumina and a large-particle thermal conductive filler; The submicron spherical γ-phase alumina has a sphericity greater than 90%, an α-phase content less than 10%, and a D50 particle size of 0.1-1 μm; The large-particle thermal conductive filler has a D50 particle size greater than 70 μm and a spherical or angular shape; The preparation method of the submicron spherical α-phase alumina specifically comprises the following steps: The submicron spherical γ-phase alumina and the large-particle thermal conductive filler are uniformly mixed; Put the evenly mixed materials into a muffle furnace for high-temperature calcination; The product obtained after calcination was wet ball milled; The ball-milled material is screened and dried to obtain submicron spherical α-phase alumina; The weight ratio of the submicron spherical γ-phase alumina to the large-particle thermal conductive filler is (20-30): (70-80); The thermal conductivity of the large-particle thermally conductive filler is greater than 20 W / (m·K), and is selected from at least one of aluminum oxide and aluminum nitride; The calcination temperature is 1200-1400° C., and the calcination time is 2-10 hours.
2. The submicron spherical α-phase alumina according to claim 1, characterized in that: The α-phase content of the submicron spherical α-phase alumina is greater than 80%.
3. The submicron spherical α-phase alumina according to claim 1, characterized in that: The large-diameter thermal conductive filler has a spherical shape.
4. The submicron spherical α-phase alumina according to claim 1, characterized in that: The wet ball milling is a stirring ball milling with a stirring frequency of 100-200 Hz, a stirring time of 10-60 min, and a powder solid content of 10-30%.
Citation Information
Patent Citations
Method for synthesizing aluminium oxide powder by using combustion method
CN106629799A
A method for preparing spherical α-phase nano-alumina
CN111484050B
Preparation method of high-purity spherical alpha-Al2O3
CN103482665A
Electronic heat conduction spherical aluminum oxide and preparation method
CN107555455A
Preparation method of low-sodium submicron calcined alumina
CN108675327A