A photocurable frame glue composition and preparation method thereof

By using photocurable frame adhesive compositions of bisphenol F-type epoxy resin and magnesium oxide, combined with the synergistic effect of sulfonium salt and anthracene photosensitizer, the frame adhesive of liquid crystal display panel under high temperature and high humidity conditions is solved. The problem of insufficient water vapor barrier and adhesion achieves efficient photocuring and sealing effects.

CN115785873BActive Publication Date: 2024-11-26XIAN AURORA NEW MATERIAL TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211574863.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-08
Publication Date
2024-11-26
Estimated Expiration
2042-12-08

AI Technical Summary

Technical Problem

The existing LCD display panel frame glue has poor water vapor barrier capacity, poor photocuring degree, weak adhesion, and other problems in high temperature and high humidity conditions, resulting in liquid crystal leakage.

Method used

The photocurable frame adhesive composition consisting of bisphenol F-type epoxy resin, boron nitride, magnesium oxide, alumina and other materials is used to synergistically act as a sulfonium salt photoinitiator and anthracene photosensitizer, and 350~ Photocuring is performed at UV wavelength of 400nm to improve curing rate and sealing properties.

Benefits of technology

It significantly improves the water vapor barrier performance and adhesion of frame adhesive under high temperature and high humidity conditions, ensures the sealing effect and flexibility of the LCD panel, and reduces production costs and complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003988926540000121
    Figure BDA0003988926540000121
Patent Text Reader

Abstract

The present invention discloses a photocurable sealant composition and a preparation method thereof. The sealant composition comprises, by weight, 60 to 80 parts of epoxy resin, 5 to 30 parts of filler, 1 to 15 parts of curing agent, and 0.1 to 5 parts of auxiliary agent; wherein the epoxy resin is preferably bisphenol F epoxy resin, the filler is a mixture of silicon dioxide and magnesium oxide, and the weight ratio of silicon dioxide to magnesium oxide is 1: (2 to 8), and the particle morphology of silicon dioxide and magnesium oxide is limited, especially the magnesium oxide is a mixture of magnesium oxide A with a certain particle size and magnesium oxide B with a specific surface area. The sealant composition of the present invention is a cationic curing system composed of epoxy resin. Under the joint action of specific fillers, sulfonium salt photoinitiators, anthracene photosensitizers, etc., curing can be completed by ultraviolet light irradiation without heating, and its curing rate is greater than 92%. At the same time, it has excellent adhesion to the substrate and excellent high temperature and high humidity resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of frame glue for liquid crystal displays, and in particular relates to a photocurable frame glue composition and a preparation method thereof. Background Art

[0002] The liquid crystal display panel is a reflective liquid crystal micro-panel that uses semiconductor silicon crystal technology to control liquid crystal and then "project" a color image. It has the characteristics of high light utilization efficiency, small size, high aperture ratio, mature manufacturing technology, etc., and can achieve high resolution and full color performance. The liquid crystal display panel includes an array substrate and a color film (CF) substrate. The two substrates are filled with liquid crystal, and a frame glue is applied around them to bond the array substrate and the CF substrate to form a display screen with a stable box thickness. The frame glue in the liquid crystal display panel mainly plays the role of bonding and sealing the upper and lower substrates of the liquid crystal box, preventing water vapor from entering, while supporting the gap between the upper and lower substrates to keep the environment inside the liquid crystal box stable and reliable. If the adhesive force of the frame glue is weak, it will cause the liquid crystal leakage during the subsequent testing and use of the liquid crystal display panel due to the separation of the frame glue.

[0003] At present, most of the fillers in the frame glue only use ordinary silicon dioxide as fillers. For example, the publication number CN106433538A discloses a visible light curing frame glue composition. With this frame glue, after the liquid crystal box is attached, it is not necessary to use ultraviolet light irradiation, and the curing reaction can be carried out under clean visible light. The filler in the frame glue composition in this special case is ordinary silicon dioxide powder, and its surface is covered with hydroxyl groups, which has certain hydrophilic properties, and its water and oxygen barrier performance is poor. In order to ensure the sealing effect, the publication number CN110903793A discloses a frame glue material and a liquid crystal display panel. In this patent, nano-inorganic substances are added to the prepolymer, and the nano-inorganic substances are uniformly dispersed in the prepolymer system. After curing, the water vapor permeation path can be extended, thereby effectively improving the water vapor barrier capacity of the frame glue under high temperature and high humidity conditions. However, in order to improve the degree of curing, this patent adopts a dual curing method of light curing and heat curing, which greatly increases the manpower and time costs. At the same time, the process yield is low, the process steps are complicated, and it is not conducive to large-scale production.

[0004] In view of this, the present inventor provides a photocurable sealant composition and a preparation method thereof to overcome the defects of the prior art. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a photocurable sealant composition and a preparation method thereof. The sealant composition solves the problems of poor water vapor barrier ability, poor photocuring degree, weak adhesion, etc. of traditional sealants under high temperature and high humidity conditions.

[0006] The objective of the present invention is achieved through the following technical solutions:

[0007] In one aspect, the present invention provides a photocurable sealant composition, which is mainly composed of the following raw materials in parts by weight:

[0008] Epoxy resin, 60-80 parts by weight;

[0009] Filler, 5 to 30 parts by weight;

[0010] Curing agent, 1 to 15 parts by weight;

[0011] Auxiliary agent, 0.1 to 5 parts by weight;

[0012] Wherein, the epoxy resin is one or more of bisphenol F epoxy resin, bisphenol A epoxy resin, bisphenol S epoxy resin or bisphenol H epoxy resin.

[0013] Preferably, the epoxy resin is bisphenol F epoxy resin.

[0014] Furthermore, the filler is one or more of boron nitride, silicon dioxide, magnesium oxide, aluminum oxide, titanium oxide, magnesium carbonate, barium sulfate, magnesium hydroxide or talc.

[0015] Furthermore, the filler is a mixture of silicon dioxide and magnesium oxide, and the weight ratio of silicon dioxide to magnesium oxide is 1:(2-8).

[0016] Preferably, the particle size of the silicon dioxide is 1 to 2 μm.

[0017] Preferably, the magnesium oxide is magnesium oxide A with a particle size of 4 to 5 μm and a specific surface area of ​​100 to 200 m 2 / g of magnesium oxide B, the weight ratio of magnesium oxide A to magnesium oxide B is 1: (0.1~10).

[0018] The magnesium oxide of the present invention adopts magnesium oxide A with a particle size of 4 to 5 μm and magnesium oxide A with a specific surface area of ​​100 to 200 m2 in a weight ratio of 1: (0.1 to 10) 2 / g of magnesium oxide B, the mixture can be evenly dispersed in the epoxy resin system, improve the sealing of the frame glue after curing, improve the water vapor barrier ability under high temperature and high humidity conditions, and at the same time improve the toughness of the frame glue after curing. After the frame glue is cured, on the one hand, part of the water vapor will react with the magnesium oxide dispersed in the epoxy resin system, blocking the further diffusion of water vapor and thus corroding the liquid crystal. The specific surface area is 100-200m 2 / g magnesium oxide B is extremely small in size. When it is evenly dispersed in the epoxy resin system, it can not only improve the sealing of the system, but also work together with magnesium oxide A with a particle size of 4 to 5μm to form a very small gap to extend the penetration path of water vapor, so that it can still effectively block water vapor under high temperature and high humidity conditions; on the other hand, the smaller magnesium oxide can penetrate into the defects of the polymer, changing the stress concentration phenomenon of the sealant, thereby improving the toughness of the sealant. In addition, when magnesium oxide A with a particle size of 4 to 5μm and a specific surface area of ​​100 to 200m 2 When the weight ratio of magnesium oxide B is too large, its water vapor isolation performance is poor. When the weight ratio of the two is too small, the specific surface area is 100-200m 2 / g of magnesium oxide B is prone to uneven dispersion and agglomeration in the epoxy resin system.

[0019] In addition, the inventors found during the experiment that when the filler is only irregularly shaped magnesium oxide, the cured sealant composition is not sufficient to support the upper and lower substrates. When silicon dioxide particles with a particle size of 1 to 2 μm are added to the system, it not only has an excellent supporting effect, but also can adjust the viscosity of the sealant composition, so that the sealant composition has excellent coating performance on the surface of the substrate. At the same time, the unique spatial network structure of silicon dioxide and the several hydroxyl groups on the surface help to enhance the interaction between silicon dioxide and bisphenol F epoxy resin molecules and the adhesion ability between the system and the substrate.

[0020] Furthermore, the curing agent is a photoinitiator and a photosensitizer.

[0021] Preferably, the photoinitiator is a cationic photoinitiator, and more preferably, the cationic photoinitiator is a sulfonium salt photoinitiator, and the added amount thereof accounts for 0.5-10% of the total weight of the frame glue composition.

[0022] Preferably, the photosensitizer is an anthracene photosensitizer, and the added amount thereof accounts for 0.1-5% of the total weight of the frame glue composition.

[0023] Furthermore, the auxiliary agent is a polyacrylate dispersant.

[0024] Furthermore, the weight ratio of the epoxy resin to the filler is (65-75):(10-25).

[0025] In a second aspect, the present invention provides an adhesive, which is prepared using the above-mentioned photocurable composition.

[0026] In a third aspect, the present invention provides a method for preparing a photocurable sealant composition, comprising the following steps:

[0027] S1. According to the raw material composition of the sealant composition, epoxy resin, filler, curing agent and auxiliary agent are mixed uniformly by weight, stirred at 60-80 rpm for 30-60 min, and then stirred at 110-140 rpm for 30-120 min to obtain a mixture;

[0028] S2. Degassing the mixture obtained in S1 using vacuum negative pressure to obtain a target sealant composition.

[0029] The sealant composition of the present invention is a photocurable composition, and uses a UV wavelength of 350 to 400 nm at 2000 to 4000 mj / cm 2 The light accumulation time is 30 to 200 seconds.

[0030] Preferably, the sealant composition uses a UV wavelength of 365 nm at 3000 mj / cm 2 The light accumulation time is 30 to 200 seconds.

[0031] Generally speaking, the ultraviolet absorption wavelength of sulfonium salt photoinitiators is relatively short, and the absorption wavelength is all below 300nm. Therefore, when the light source in the present invention is ultraviolet light with a wavelength of 365nm, the sulfonium salt photoinitiator will fail. For this reason, the present invention uses a photosensitizer containing an anthracene skeleton, which has a higher light absorption intensity at a wavelength of 365nm, effectively improving the photopolymerization speed of the epoxy resin and the curing rate of the frame glue composition. This is because the anthracene photosensitizer with a sensitizing effect has a stronger electron donating ability and can produce a larger concentration of active cations. After being excited by the light source of about 365nm, it interacts with the sulfonium salt photoinitiator, promotes the decomposition of the sulfonium salt photoinitiator, generates a cationic polymer initiation active center, promotes the increase of the epoxy conversion rate of the bisphenol F epoxy resin polymerization, and improves the photocuring rate of the frame glue composition. At the same time, after extensive research by the inventors, it was found that when the cumulative amount of light is 3000mj / cm 2 When the adhesive composition has the best adhesion to the substrate.

[0032] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:

[0033] 1. The present invention adopts a mixture of silicon dioxide and magnesium oxide of different sizes in a weight ratio of 1: (2 to 8) as a filler, which can be evenly dispersed in bisphenol F epoxy resin and improve the sealing property of the cured sealant composition, thereby significantly improving the water vapor barrier performance and the adhesion ability with the substrate under high temperature and high humidity conditions, and at the same time improving the flexibility of the sealant composition.

[0034] 2. The present invention uses the synergistic effect of sulfonium salt photoinitiator and anthracene photosensitizer to utilize UV ​​wavelength of 350-400nm with 2000-4000mj / cm2 The light cumulative amount of curing can effectively improve the light curing rate of the frame glue composition, and at the same time, the adhesion between the frame glue composition and the substrate is also significantly improved.

[0035] 3. The present invention adopts polyacrylate dispersants and utilizes the steric hindrance provided by the long chain structure of polyacrylates to improve the dispersion stability of the filler and avoid the slippage of silicon dioxide ions during the subsequent preparation and lamination process of the liquid crystal display panel.

[0036] 4. The present invention uses a cationic curing system composed of epoxy resin only. Under the action of sulfonium salt photoinitiator and anthracene photosensitizer, curing can be completed only by ultraviolet light irradiation without heating. The actual verification shows that the curing rate is greater than 92%, which ensures the support capacity and sealing effect of the sealant composition. In addition, the hydroxyl groups generated by the bisphenol F epoxy resin after curing and ring opening can further improve the adhesion of the sealant composition to the substrate. DETAILED DESCRIPTION

[0037] Here, exemplary embodiments will be described in detail. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Instead, they are only examples consistent with some aspects of the present invention as detailed in the appended claims.

[0038] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with embodiments.

[0039] Example 1

[0040] The photocurable sealant composition provided in this embodiment comprises, by weight, 70 parts of resin, 20 parts of filler, 7 parts of curing agent, and 3 parts of auxiliary agent.

[0041] Specifically, the epoxy resin is bisphenol F diglycidyl ether epoxy resin, CAS No.: 2095-03-6, purchased from Guangdong Wengjiang Chemical Reagent Co., Ltd.

[0042] The filler is a mixture of silicon dioxide and magnesium oxide, with a weight ratio of 1:4. The silicon dioxide has a particle size of 2 μm, CAS number 60676-86-0, purchased from McLean; the magnesium oxide is magnesium oxide A with a particle size of 5 μm and a specific surface area of ​​150 m 2 / g of magnesium oxide B, the weight ratio of magnesium oxide A to magnesium oxide B is 1:1. Magnesium oxide A with a particle size of 5 μm was purchased from ZH-V2-2 of Jiangsu Zehui Magnesium-based New Material Technology Co., Ltd.; the specific surface area is 150 m 2 / g of magnesium oxide B was purchased from ZH-V150 of Jiangsu Zehui Magnesium-based New Material Technology Co., Ltd.

[0043] The curing agent is a mixture of triaryl hexafluoroantimonate sulfonium salt and 9,10-dibutoxyanthracene, with a weight ratio of 5:2. Among them, triaryl hexafluoroantimonate sulfonium salt was purchased from Changzhou Qiangli Electronic New Materials Co., Ltd. TR-PAG-201; 9,10-dibutoxyanthracene was purchased from Changzhou Qiangli Electronic New Materials Co., Ltd. TR-PSS-303.

[0044] The additive is a polyacrylate dispersant purchased from BYK2001.

[0045] This embodiment provides a method for preparing a photocurable sealant composition, and the specific steps are as follows:

[0046] 1) According to the raw material composition of the above-mentioned sealant composition, epoxy resin, filler, curing agent and auxiliary agent are mixed uniformly according to weight parts, stirred at 70 rpm for 40 minutes, and then stirred at 120 rpm for 60 minutes to obtain a mixture;

[0047] 2) The mixture obtained in 1) is subjected to a vacuum degassing treatment to obtain a target sealant composition.

[0048] Example 2

[0049] The photocurable sealant composition provided in this embodiment comprises, by weight, 78 parts of resin, 30 parts of filler, 10 parts of curing agent, and 5 parts of auxiliary agent.

[0050] Specifically, the epoxy resin is bisphenol F diglycidyl ether epoxy resin, CAS No.: 2095-03-6, purchased from Guangdong Wengjiang Chemical Reagent Co., Ltd.

[0051] The filler is a mixture of silicon dioxide and magnesium oxide, with a weight ratio of 1:8. The silicon dioxide has a particle size of 2 μm, CAS number 60676-86-0, purchased from McLean; the magnesium oxide is magnesium oxide A with a particle size of 5 μm and a specific surface area of ​​150 m 2 / g of magnesium oxide B, the weight ratio of magnesium oxide A to magnesium oxide B is 1:1. Magnesium oxide A with a particle size of 5 μm was purchased from ZH-V2-2 of Jiangsu Zehui Magnesium-based New Material Technology Co., Ltd.; the specific surface area is 150 m 2 / g of magnesium oxide B was purchased from ZH-V150 of Jiangsu Zehui Magnesium-based New Material Technology Co., Ltd.

[0052] The curing agent is a mixture of triaryl hexafluoroantimonate sulfonium salt and 9,10-dibutoxyanthracene, with a weight ratio of 7:3. Among them, triaryl hexafluoroantimonate sulfonium salt was purchased from Changzhou Qiangli Electronic New Materials Co., Ltd. TR-PAG-201; 9,10-dibutoxyanthracene was purchased from Changzhou Qiangli Electronic New Materials Co., Ltd. TR-PSS-303.

[0053] The additive is a polyacrylate dispersant purchased from BYK2001.

[0054] This embodiment provides a method for preparing a photocurable sealant composition, and the specific steps are as follows:

[0055] 1) According to the raw material composition of the above-mentioned sealant composition, epoxy resin, filler, curing agent and auxiliary agent are mixed uniformly according to weight parts, stirred at 60 rpm for 60 min, and then stirred at 140 rpm for 40 min to obtain a mixture;

[0056] 2) The mixture obtained in 1) is subjected to a vacuum degassing treatment to obtain a target sealant composition.

[0057] Example 3

[0058] The photocurable sealant composition provided in this embodiment comprises, by weight, 60 parts of resin, 8 parts of filler, 6 parts of curing agent, and 2 parts of auxiliary agent.

[0059] Specifically, the epoxy resin is bisphenol F diglycidyl ether epoxy resin, CAS No.: 2095-03-6, purchased from Guangdong Wengjiang Chemical Reagent Co., Ltd.

[0060] The filler is a mixture of silicon dioxide and magnesium oxide, with a weight ratio of 1:2. The silicon dioxide has a particle size of 2 μm, CAS number 60676-86-0, purchased from McLean; the magnesium oxide is magnesium oxide A with a particle size of 5 μm and a specific surface area of ​​150 m 2 / g of magnesium oxide B, the weight ratio of magnesium oxide A to magnesium oxide B is 1:1. Magnesium oxide A with a particle size of 5 μm was purchased from ZH-V2-2 of Jiangsu Zehui Magnesium-based New Material Technology Co., Ltd.; the specific surface area is 150 m 2 / g of magnesium oxide B was purchased from ZH-V150 of Jiangsu Zehui Magnesium-based New Material Technology Co., Ltd.

[0061] The curing agent is a mixture of triaryl hexafluoroantimonate sulfonium salt and 9,10-dibutoxyanthracene, with a weight ratio of 4:2. Among them, triaryl hexafluoroantimonate sulfonium salt was purchased from Changzhou Qiangli Electronic New Materials Co., Ltd. TR-PAG-201; 9,10-dibutoxyanthracene was purchased from Changzhou Qiangli Electronic New Materials Co., Ltd. TR-PSS-303.

[0062] The additive is a polyacrylate dispersant purchased from BYK2001.

[0063] This embodiment provides a method for preparing a photocurable sealant composition, and the specific steps are as follows:

[0064] 1) According to the raw material composition of the above-mentioned sealant composition, epoxy resin, filler, curing agent and auxiliary agent are mixed uniformly according to weight parts, stirred at 80 rpm for 50 min, and then stirred at 110 rpm for 100 min to obtain a mixture;

[0065] 2) The mixture obtained in 1) is subjected to a vacuum degassing treatment to obtain a target sealant composition.

[0066] Comparative Example 1

[0067] The difference from Example 1 is that the filler in Comparative Example 1 is magnesium oxide A with a particle size of 5 μm and a specific surface area of ​​150 m 2 / g of magnesium oxide B, the weight ratio is 1:1, only silicon dioxide is not added.

[0068] Comparative Example 2

[0069] Different from Example 1, the filler in Comparative Example 2 is a mixture of silicon dioxide and magnesium oxide, with a weight ratio of 1:4, wherein the magnesium oxide is only magnesium oxide A with a particle size of 5 μm.

[0070] Comparative Example 3

[0071] Different from Example 1, the curing agent in Comparative Example 3 is a mixture of triaryl hexafluoroantimonate sulfonium salt and 2,4,6-trimethylbenzophenone, with a weight ratio of 5:2. Among them, triaryl hexafluoroantimonate sulfonium salt was purchased from Changzhou Qiangli Electronic New Materials Co., Ltd. TR-PAG-201; 2,4,6-trimethylbenzophenone was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.

[0072] Performance Test:

[0073] The photocurable sealant compositions obtained in Examples 1 to 3 and Comparative Examples 1 to 3 were spin-coated on a glass substrate and irradiated with a UV wavelength of 365 nm at 3000 mj / cm 2 The sample with a thickness of 13 μm was obtained by curing for 160 s with the light accumulation amount of .

[0074] (1) Adhesion: Use a grid cutting disc and a utility knife to cut the sample into grids. Stick 3M transparent tape on the grids and apply force to make the tape firmly adhere to the sample surface and the grids. Within 1 to 2 minutes, hold one end of the 3M tape at an angle of 60 degrees and press it at 0.5 -1 The tape can be peeled off smoothly within seconds. Visually inspect the peeling phenomenon and degree of the coating on the substrate to determine its ASTM grade.

[0075] ASTM grade: 5B-the cut edge is smooth, and there is no peeling on the grid edge; 4B-the peeling area in the cross-cut area is ≤5%; 3B-the peeling area in the cross-cut area is greater than 5% to 15%; 2B-the peeling area in the cross-cut area is greater than 15% to 35%; 1B-the peeling area in the cross-cut area is greater than 35% to 65%; 0B-the peeling area in the cross-cut area is greater than 65%.

[0076] (2) Curing rate: The curing rate of the photocurable sealant composition before and after curing was measured using FT-IR (Nicolet iS50, Thermo-Fisher) at 1635 cm -1 (C=C) and 1720cm -1 Absorption peak intensity near (C=O).

[0077] Photocuring rate (%) = |1-(F / S)|x100;

[0078] Wherein, F is the photocurable sealant composition after curing at 1635cm -1 The absorption peak intensity near 1720cm -1 The ratio of the absorption peak intensities near 1635cm -1 The absorption peak intensity near 1720cm -1 The ratio of the absorption peak intensities near

[0079] (3) High temperature and high humidity resistance: The prepared cured photocurable sealant composition was subjected to water vapor transmission rate testing at 85° C. and 85% relative humidity for 90 hours using a water vapor transmission rate tester (PERMATRAN-W3 / 33, manufactured by MOCON).

[0080] The performance test results are shown in Table 1 below.

[0081] Table 1

[0082]

[0083] It can be seen from the test results in Table 1 that the sealant composition prepared by the present invention has excellent adhesion to the substrate, high curing rate, and excellent high temperature and high humidity resistance. According to the test results of Comparative Examples 1 and 2, when the filler lacks silicon dioxide or magnesium oxide A with a particle size of only 5 μm, its adhesion and high temperature and high humidity resistance cannot achieve the desired effect, which further proves the rationality of the formula of the present invention. In addition, when 2,4,6-trimethylbenzophenone in Comparative Example 3 is a benzophenone photosensitizer instead of anthracene photosensitizer, its photocuring rate is low, resulting in low water vapor permeability.

[0084] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention.

[0085] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.

Claims

1. A photocurable sealant composition, characterized in that: The sealant composition is mainly composed of the following raw materials by weight: composition: Epoxy resin, 60-80 parts by weight; Filler, 5 to 30 parts by weight; Curing agent, 1 to 15 parts by weight; Auxiliary agent, 0.1 to 5 parts by weight; The epoxy resin is one or more of bisphenol F epoxy resin, bisphenol A epoxy resin, bisphenol S epoxy resin or bisphenol H epoxy resin; the filler is a mixture of silicon dioxide and magnesium oxide, and the weight ratio of silicon dioxide to magnesium oxide is 1: (2-8); The particle size of the silicon dioxide is 1 to 2 μm; The magnesium oxide is a mixture of magnesium oxide A with a particle size of 4 to 5 μm and magnesium oxide B with a specific surface area of ​​100 to 200 m2 / g, and the weight ratio of magnesium oxide A to magnesium oxide B is 1:(0.1 to 10); The curing agent is a photoinitiator and a photosensitizer, the photoinitiator is a cationic photoinitiator, and the photosensitizer is an anthracene photosensitizer.

2. A photocurable sealant composition according to claim 1, characterized in that: The cationic photoinitiator is added in an amount of 0.5-10% of the total weight of the sealant composition.

3. The photocurable sealant composition according to claim 1, characterized in that: The amount of the anthracene photosensitizer added is 0.1-5% of the total weight of the sealant composition.

4. The photocurable sealant composition according to claim 1, characterized in that: The auxiliary agent is a polyacrylate dispersant.

5. The photocurable sealant composition according to claim 1, characterized in that: The weight ratio of the epoxy resin to the filler is (65-75): (10-25).

6. The method for preparing the photocurable sealant composition according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1. According to the raw material composition of the sealant composition, epoxy resin, filler, curing agent and auxiliary agent are mixed uniformly by weight, stirred at 60-80 rpm for 30-60 min, and then stirred at 110-140 rpm for 30-120 min to obtain a mixture; S2. Degassing the mixture obtained in S1 using vacuum negative pressure to obtain a target sealant composition.

Citation Information

Patent Citations

  • Visible light curing type frame seal adhesive composition

    CN106433538A

  • Frame sealing adhesive material and liquid crystal display panel

    CN110903793A

  • High-Tg, high-adhesion and aging-resistant epoxy adhesive composition as well as preparation method and application thereof

    CN115029089A

  • Dual-sensitized cationic epoxy adhesive as well as preparation method and application thereof

    CN115260960A

  • Photo-induced cation curable epoxy resin composition

    US20050245643A1