Meta-aramid fiber with concentrated length distribution and high water retention value and preparation method thereof

The aramid decomposition fibers are processed through the refining, dispersing and sieving processes, which solves the problem of inconcentrated length distribution, achieves high water retention value and uniform film structure, improves the density and electrical performance of the paper, and meets the high-end Technical requirements for application.

CN115787123BActive Publication Date: 2024-11-15ZHUZHOU TIMES FIBER PIONEER MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211132143.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-16
Publication Date
2024-11-15
Estimated Expiration
2042-09-16

AI Technical Summary

Technical Problem

In the prior art, the length distribution of aramid decomposition fibers is not concentrated, resulting in poor paper bonding ability and poor paper uniformity, and the preparation method for high water retention value decomposition fibers has not been effectively solved.

Method used

The process of decomposing crude fibers is processed by combining refining, dissolution and sieving. By regulating the logarithmic viscosity and process parameters of polymer concentration, the fiber length distribution is controlled, excessively long fibers and crude fibers are removed, and the film shape is improved uniform. , obtain high water retention value deposition fibers with concentrated length distribution.

Benefits of technology

It significantly improves the density, tensile strength and electrical strength of the paper, reaches the level of imported products, meets the technical requirements of honeycomb paper for aerospace, and improves the dispersion and water retention value of the settled fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention provides a method for preparing meta-aramid fibrids with a concentrated length distribution and a high water retention value, comprising the following steps: (1) preparing a meta-aramid resin solution, wherein the polymer content of the meta-aramid resin solution is 6% to 14%, the inherent viscosity is 1.5 to 1.8 dL / g, and the temperature is 40°C to 70°C; (2) injecting the meta-aramid resin solution and a precipitating agent into a precipitator, precipitating and cooling to form, obtaining a crude fibrid product, and subjecting the crude fibrid product to pulping, debonding, and sieving to obtain a fibrid slurry; (3) washing the fibrid slurry to obtain meta-aramid fibrids with a concentrated length distribution and a high water retention value. The fibrids prepared in the present application have a high water retention value, good dispersibility, a uniform film structure, and a concentrated length distribution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of synthetic fibers, and in particular relates to a meta-aramid fibrid and a preparation method thereof. Background Art

[0002] Aramid paper-based materials have excellent thermal stability, flame retardancy, electrical insulation, etc., and have become important basic materials in the fields of rail transportation, aerospace, national defense and military industry. Meta-aramid paper is made of chopped fibers and precipitated fibers through wet papermaking and hot pressing. Chopped fibers mainly provide mechanical properties and play a role in skeleton support, while precipitated fibers mainly provide insulation properties and play a role in entanglement and bonding. Precipitated fibers usually account for more than 50% of meta-aramid paper and are the key intermediate raw materials in the entire meta-aramid industry chain.

[0003] At present, the high-performance aramid paper-based materials needed in China still rely mainly on imports. DuPont, relying on its technological advantages, does not sell precipitated fibers separately, but only sells them in the form of aramid paper or aramid products. It completely monopolizes the high-end market of aramid materials. It can be seen that the morphology and performance of precipitated fibers are important for the preparation of aramid paper-based materials. At present, the research on precipitated fibers at home and abroad mainly focuses on the improvement of precipitation equipment and precipitation process, but there are few reports on the control of precipitated fiber morphology and its influence on product performance. The aramid precipitated fibers prepared by the existing process have the disadvantages of less film-like structure, large fiber morphology difference, and non-concentrated length distribution, which directly leads to poor paper bonding ability and poor paper uniformity. Therefore, how to provide a film-like precipitated fiber with concentrated length distribution has become a technical problem that needs to be urgently solved in the preparation of high-performance aramid paper.

[0004] The invention patent with application number CN201510012906.X discloses a method for preparing aromatic polyamide precipitated fibers. The main difference lies in the use of a precipitated solvent mixed with water, DMAC and chloride salt, especially the addition of chloride salt formula, which is conducive to the formation of film-like or fibrous precipitated fibers.

[0005] The invention patent with application number CN201910543968.1 provides a method for preparing wide film-like precipitated fibers. Its main feature is that the precipitated fiber solvent mixture coming out of the high-speed shearing equipment is passed through a special disc grinder to further stretch and solidify the morphology of the precipitated fiber membrane, thereby forming precipitated fibers with rich hairiness and wide film-like morphology.

[0006] The invention patent with application number CN2020104029288 discloses a method for preparing aromatic polyamide membrane-like precipitated fibers. The difference lies in that the polymer solution flows out from a flat spinneret and passes through an air layer, so that the polymer solution flow forms a ribbon-shaped solution "flow" before entering the coagulation bath. The ribbon-shaped solution "flow" is further stretched and deformed into a membrane-like precipitated fiber under the strong shearing action of the coagulation bath. The structure is uniform, membrane-like, and the length distribution is relatively concentrated.

[0007] Both patents with application numbers CN201510012906.X and CN201910543968.1 do not involve the control of the length distribution of fibrils. The fibrils prepared in the implementation cases of patent CN201510012906.X have low beating degrees, which do not exceed 40°SR. The bonding performance is poor when combined with short-cut fibers, the paper structure is not dense, and the mechanical properties and electrical insulation properties are not good. Patent CN201910543968.1 uses a specific disc grinder to grind the fibril solvent mixture to further stretch and membrane the fibrils, but the cutting of the fibrils is not much. The prepared fibrils have a Schober beating degree of only 45-60°SR, which is not suitable for high-end applications with high requirements for electrical insulation performance or low requirements for paper permeability. Secondly, the coagulation liquid used in the invention is a mixture of amide solvents, alcohol solvents and water. The introduction of alcohol solvents increases the cost of solvent recovery. Patent CN2020104029288 mainly controls the size and specific surface area of ​​precipitated fibers by adjusting the shape and size of the spinneret and the height of the air layer, so that more than 70% of the length distribution of precipitated fibers is concentrated within a certain range, but does not accurately control the proportion of fibers with a length of less than 0.2 mm (referred to as fine fibers) and the proportion of fibers with a length of more than 2.0 mm (referred to as overlong fibers). Too high a proportion of fine fibers will affect the binding ability of paper, and too high a proportion of overlong fibers will easily entangle with short-cut fibers to form pulp clumps, affecting the uniformity of paper. In addition, this invention patent controls the concentrated distribution of the length of precipitated fibers by adjusting the precipitation process parameters, but it cannot achieve precise control of each length interval. No reports have been found so far on the use of a special process combining refining, debonding, and screening for the initial product of precipitated fibers to control the length of precipitated fibers, reduce the proportion of overlong fibers, improve the membrane structure, and achieve concentrated length distribution and high water retention value precipitated fiber preparation. Summary of the invention

[0008] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the above background technology and provide a meta-aramid fiber with concentrated length distribution and high water retention value and a preparation method thereof.

[0009] In order to solve the above technical problems, the technical solution proposed by the present invention is:

[0010] A method for preparing meta-aramid fibrid with concentrated length distribution and high water retention value comprises the following steps:

[0011] (1) preparing a meta-aramid resin solution, wherein the aramid resin solution has a polymer content of 6% to 14%, a logarithmic viscosity of 1.5 to 1.8 dL / g, and a temperature of 40° C. to 70° C.;

[0012] (2) injecting the meta-aramid resin solution and the precipitating agent into a precipitator, precipitating and cooling to form, to obtain a crude fibrillation product, and the crude fibrillation product is subjected to pulping, debonding, and sieving to obtain a fibrillation slurry;

[0013] (3) washing the precipitated fiber slurry to obtain meta-aramid fiber precipitated with concentrated length distribution and high water retention value.

[0014] The crude fibrillation product is treated by a refiner to remove overlong fibers, by a deflaker to further stretch the product and obtain a more film-like form, and by a pressure screen to remove pulp particles and coarse fibers, thereby obtaining a fibrillation slurry with uniform length distribution and free of impurities.

[0015] The higher the logarithmic viscosity of the meta-aramid resin, the lower the polymer content in the resin or the higher the temperature. By adjusting the above three parameters, the morphology of the crude fiber precipitation product can be controlled.

[0016] The combined treatment of refining-flushing-screening is adopted. If the post-treatment (refining-flushing-screening) is not adopted, the fiber length is long and the distribution is not concentrated, the beating degree is low, the paper uniformity is not good, and the breakdown voltage is not high. Refining is mainly to remove the overlong fibers, flushing is mainly to improve the film structure, and screening is to remove the coarse fibers or small pulp agglomerates.

[0017] Preferably, the preparation of the meta-aramid resin solution in step (1) is specifically as follows: meta-phenylenediamine and isophthaloyl chloride are polymerized in an amide solvent, neutralized and filtered to obtain a meta-aramid resin stock solution, and then diluted and stirred to obtain a meta-aramid resin solution.

[0018] Preferably, the precipitating agent in step (2) is an amide solvent, the mass content is 25% to 50%, and the temperature is 0°C to 30°C.

[0019] Preferably, the amide solvent is N,N-dimethylformamide and / or N,N-dimethylacetamide.

[0020] Preferably, in step (2), the meta-aramid resin solution and the precipitating agent are injected into the precipitator through a spinneret hole, the spinneret hole is rectangular, 0.5 to 5 mm long and 0.05 to 1 mm wide; the precipitator comprises a stator and a rotor, the spacing between the spinneret hole and the rotor is 0.2 to 1.0 mm, and the spacing between the stator and the rotor is 0.2 to 1.0 mm.

[0021] Preferably, the volume ratio of the meta-aramid resin solution to the precipitant in step (2) is 1:10-25, and the precipitator speed is 3000-6000 rpm. The intrinsic viscosity of the meta-precipitated aramid resin is small, and a relatively small speed is required to achieve a good precipitation and dispersion effect.

[0022] Preferably, the refining in step (2) is performed by cone milling, the refining power is 150-250 kW, and the refining time is 20-60 min.

[0023] Preferably, the precipitated fiber slurry in step (2) has a logarithmic viscosity of 1.5 to 1.8 dL / g, a beating degree of 65 to 85oSR, a weight-average length of 0.7 to 1.0 mm, a width greater than 23 μm, a proportion of overlong fibers less than 1.0%, a proportion of fine fibers less than 10%, and a water retention value greater than 300%.

[0024] Under the same technical concept, the present invention also provides a meta-aramid fiber with a concentrated length distribution and a high water retention value, wherein the residual solvent in the fiber is less than 100 ppm.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] (1) The precipitated fibrils prepared in the present application have high water retention value, good dispersibility, uniform film structure and concentrated length distribution.

[0027] (2) The preparation method of the present application adopts a combination of precipitation-refining-fluffing-screening steps to control the morphology of the precipitated fibers; an aramid resin solution with a suitable relative logarithmic viscosity is used in combination with a spinneret of a specific size, and by controlling the distance between the rotor and the stator, and the distance between the nozzle and the rotor, a crude precipitated fiber product with a small proportion of overlong fibers and a small proportion of fine fibers can be obtained; a combination of refining-fluffing-screening is used to control the refining process parameters, and the crude precipitated fiber product is subjected to uniformity and further membrane treatment, thereby obtaining precipitated fibers with a suitable length and concentrated length distribution and a high water retention value.

[0028] (3) When the fibrids prepared by the present invention are combined with short-cut fibers to form paper, the paper sheet density and paper uniformity can be significantly improved, and the paper tensile strength and electrical strength can be significantly improved, reaching the level of imported products. 2Aramid paper has an air permeability as low as 0.02μm / (Pa·s), a dense paper structure, and the honeycomb will not become brittle after being dipped in glue. It can meet the technical requirements of honeycomb paper for aerospace use and fill in the domestic gap. DETAILED DESCRIPTION

[0029] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and carefully in combination with preferred embodiments below, but the protection scope of the present invention is not limited to the following specific embodiments.

[0030] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0031] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0032] Embodiment 1:

[0033] (1) m-phenylenediamine and isophthaloyl chloride are polymerized in DMAC, and the inherent viscosity of the polymer is controlled to be 1.6 dL / g. After neutralization and filtration, a meta-aramid resin stock solution is obtained, which is then diluted, stirred, and kept warm to obtain a 50°C meta-aramid resin solution with a polymer solid content of 7%.

[0034] (2) Mix water and DMAC, wherein the DMAC content is 35%, stir evenly, and cool the precipitant to 20° C. for use.

[0035] (3) The meta-aramid resin solution and the precipitating agent were injected into a high-speed rotating disc precipitator in a volume ratio of 1:15, wherein the aramid resin solution was injected through a 3.0 mm*0.2 mm spinneret hole, the distance between the nozzle and the rotor was 0.5 mm, the distance between the stator and the rotor was 0.3 mm, and the precipitator speed was 5000 rpm. The precipitate was discharged into a storage tank through the discharge port and placed overnight, and further cooled and formed to obtain a crude precipitated fiber product with a beating degree of 63°SR. The crude product was processed by cone milling, the mill power was 160 kW, the refining time was 48 min, and then after sufficient delamination and screening, a precipitated fiber slurry with a beating degree of 71°SR was obtained.

[0036] (4) The precipitated fibrillation slurry was repeatedly washed with water in a belt washer to obtain a precipitated fibrillation product with a DMAC content of 10.0 ppm. The length distribution parameters and water retention value of the finished product were tested.

[0037] (5) The obtained precipitated fiber product and short-cut fiber were mixed at a pressure of 28 g / m 2 After papermaking, hot pressing is performed to test the air permeability, tensile strength and electrical strength of the paper sample.

[0038] Embodiment 2:

[0039] (1) m-phenylenediamine and isophthaloyl chloride are polymerized in DMAC, and the inherent viscosity of the polymer is controlled to be 1.8 dL / g. After neutralization and filtration, a meta-aramid resin stock solution is obtained, which is then diluted, stirred, and kept warm to obtain a 60°C meta-aramid resin solution with a polymer solid content of 8%.

[0040] (2) Mix water and DMAC, wherein the DMAC content is 30%, stir evenly, and cool the precipitant to 10° C. for use.

[0041] (3) The meta-aramid resin solution and the precipitating agent are injected into a high-speed rotating disc precipitator in a volume ratio of 1:18, wherein the aramid resin solution is injected through a 2.0 mm*0.1 mm spinneret hole, the distance between the nozzle and the rotor is 0.4 mm, the distance between the stator and the rotor is 0.5 mm, and the precipitator speed is 6000 rpm. The precipitate is discharged into a storage tank through the discharge port and placed overnight, and further cooled and formed to obtain a crude precipitated fiber product with a beating degree of 67°SR. The crude product is processed by cone milling, the mill power is 180 kW, the refining time is 40 min, and then after sufficient delamination and screening, a precipitated fiber slurry with a beating degree of 75°SR is obtained.

[0042] (4) The precipitated fibrillation slurry was repeatedly washed with water in a belt washer to obtain a precipitated fibrillation product with a DMAC content of 12.6 ppm. The length distribution parameters and water retention value of the finished product were tested.

[0043] (5) The obtained precipitated fiber product and short-cut fiber were mixed at a pressure of 28 g / m 2 After papermaking, hot pressing is performed to test the air permeability, tensile strength and electrical strength of the paper sample.

[0044] Embodiment 3:

[0045] (1) Metaphenylenediamine and isophthaloyl chloride are polymerized in DMAC to control the inherent viscosity of the polymer to be 1.7 dL / g. After neutralization and filtration, a meta-aramid resin stock solution is obtained. The meta-aramid resin solution having a polymer solid content of 10% at 70° C. is then obtained by dilution, stirring and heat preservation.

[0046] (2) Mix water and DMAC, wherein the DMAC content is 28%, stir evenly, and cool the precipitant to 15° C. for use.

[0047] (3) The meta-aramid resin solution and the precipitating agent were injected into a high-speed rotating disc precipitator in a volume ratio of 1:16, wherein the aramid resin solution was injected through a 3.0 mm*0.15 mm spinneret hole, the distance between the nozzle and the rotor was 0.3 mm, the distance between the stator and the rotor was 0.8 mm, and the precipitator speed was 3000 rpm. The precipitate was discharged into a storage tank through the discharge port and placed overnight, and further cooled and formed to obtain a crude precipitated fiber product with a beating degree of 68°SR. The crude product was processed by cone milling, the mill power was 200 kW, the refining time was 30 min, and then after sufficient delamination and screening, a precipitated fiber slurry with a beating degree of 77°SR was obtained.

[0048] (4) The fibrid slurry was repeatedly washed with water in a belt washer to obtain a fibrid product with a DMAC content of 51.0 ppm. The length distribution parameters and water retention value of the finished product were tested.

[0049] (5) The obtained precipitated fiber product and short-cut fiber were mixed at a pressure of 28 g / m 2 After papermaking, hot pressing is performed to test the air permeability, tensile strength and electrical strength of the paper sample.

[0050] Embodiment 4:

[0051] (1) Metaphenylenediamine and isophthaloyl chloride are polymerized in DMAC, and the inherent viscosity of the polymerization is controlled to be 1.6 dL / g. After neutralization and filtration, a meta-aramid resin stock solution is obtained, which is then diluted, stirred, and kept warm to obtain a meta-aramid resin solution at 40° C. with a polymer solid content of 9%.

[0052] (2) Mix water and DMAC, wherein the DMAC content is 40%, stir evenly, and cool the precipitant to 10° C. for use.

[0053] (3) The meta-aramid resin solution and the precipitating agent are injected into a high-speed rotating disc precipitator in a volume ratio of 1:12, wherein the aramid resin solution is injected through a 1.0 mm*0.1 mm spinneret hole, the distance between the nozzle and the rotor is 0.4 mm, the distance between the stator and the rotor is 0.4 mm, and the precipitator speed is 4000 rpm. The precipitate is discharged into a storage tank through the discharge port and placed overnight, and further cooled and formed to obtain a crude precipitated fiber product with a beating degree of 72°SR. The crude product is processed by cone milling, the mill power is 210 kw, the refining time is 25 minutes, and then after sufficient delamination and screening, a precipitated fiber slurry with a beating degree of 80°SR is obtained.

[0054] (4) The precipitated fibrillation slurry was repeatedly washed with water in a belt washer to obtain a precipitated fibrillation product with a DMAC content of 10.0 ppm. The length distribution parameters and water retention value of the finished product were tested.

[0055] (5) The obtained precipitated fiber product and short-cut fiber were mixed at a pressure of 28 g / m 2After papermaking, hot pressing is performed to test the air permeability, tensile strength and electrical strength of the paper sample.

[0056] Comparative Example 1:

[0057] (1) m-phenylenediamine and isophthaloyl chloride are polymerized in DMAC, and the inherent viscosity of the polymer is controlled to be 1.6 dL / g. After neutralization and filtration, a meta-aramid resin stock solution is obtained, which is then diluted, stirred, and kept warm to obtain a 50°C meta-aramid resin solution with a polymer solid content of 7%.

[0058] (2) Mix water and DMAC, wherein the DMAC content is 35%, stir evenly, and cool the precipitant to 20° C. for use.

[0059] (3) The meta-aramid resin solution and the precipitant were injected into a high-speed rotating disc precipitator at a volume ratio of 1:15, wherein the aramid resin solution was injected through a 3.0 mm*0.2 mm spinneret hole, the distance between the nozzle and the rotor was 0.5 mm, the distance between the stator and the rotor was 0.3 mm, and the precipitator speed was 5000 rpm. The precipitate was discharged into a storage tank through the discharge port and placed overnight, and further cooled and formed to obtain a crude precipitated fiber product with a beating degree of 63°SR.

[0060] (4) The precipitated fibrillation slurry was repeatedly washed with water in a belt washer to obtain a precipitated fibrillation product with a DMAC content of 38.2 ppm. The length distribution parameters and water retention value of the finished product were tested.

[0061] (6) The obtained precipitated fiber product and short-cut fiber were mixed at a pressure of 28 g / m 2 After papermaking, hot pressing is performed to test the air permeability, tensile strength and electrical strength of the paper sample.

[0062] Comparative Example 2:

[0063] (1) m-phenylenediamine and isophthaloyl chloride are polymerized in DMAC, and the inherent viscosity of the polymer is controlled to be 1.8 dL / g. After neutralization and filtration, a meta-aramid resin stock solution is obtained, which is then diluted, stirred, and kept warm to obtain a 60°C meta-aramid resin solution with a polymer solid content of 8%.

[0064] (2) Mix water and DMAC, wherein the DMAC content is 30%, stir evenly, and cool the precipitant to 10° C. for use.

[0065] (3) The meta-aramid resin solution and the precipitating agent are injected into a high-speed rotating disc precipitator in a volume ratio of 1:18, wherein the aramid resin solution is injected through a 2.0 mm*0.1 mm spinneret hole, the distance between the nozzle and the rotor is 2.0 mm, the distance between the stator and the rotor is 1.5 mm, and the precipitator speed is 6000 rpm. The precipitate is discharged into a storage tank through the discharge port and placed overnight, and further cooled and formed to obtain a crude precipitated fiber product with a beating degree of 59°SR. The crude product is processed by cone milling, the mill power is 180 kW, the refining time is 40 min, and then after sufficient delamination and screening, a precipitated fiber slurry with a beating degree of 68°SR is obtained.

[0066] (4) The precipitated fibrillation slurry was repeatedly washed with water in a belt washer to obtain a precipitated fibrillation product with a DMAC content of 10.5 ppm. The length distribution parameters and water retention value of the finished product were tested.

[0067] (5) The obtained precipitated fiber product and short-cut fiber were mixed at a pressure of 28 g / m 2 After papermaking, hot pressing is performed to test the air permeability, tensile strength and electrical strength of the paper sample.

[0068] Comparative Example 3:

[0069] (1) m-phenylenediamine and isophthaloyl chloride are polymerized in DMAC, and the inherent viscosity of the polymer is controlled to be 1.0 dL / g. After neutralization and filtration, a meta-aramid resin stock solution is obtained, which is then diluted, stirred, and kept warm to obtain a 70°C meta-aramid resin solution with a polymer solid content of 10%.

[0070] (2) Mix water and DMAC, wherein the DMAC content is 28%, stir evenly, and cool the precipitant to 15° C. for use.

[0071] (3) The meta-aramid resin solution and the precipitating agent were injected into a high-speed rotating disc precipitator in a volume ratio of 1:16, wherein the aramid resin solution was injected through a 3.0 mm*0.15 mm spinneret hole, the distance between the nozzle and the rotor was 0.3 mm, the distance between the stator and the rotor was 0.8 mm, and the precipitator speed was 3000 rpm. The precipitate was discharged into a storage tank through the discharge port and placed overnight, and further cooled and formed to obtain a crude precipitated fiber product with a beating degree of 57°SR. The crude product was processed by cone milling, the mill power was 200 kW, the refining time was 30 min, and then after sufficient delamination and screening, a precipitated fiber slurry with a beating degree of 65°SR was obtained.

[0072] (4) The precipitated fibrillation slurry was repeatedly washed with water in a belt washer to obtain a precipitated fibrillation product with a DMAC content of 19.5 ppm. The length distribution parameters and water retention value of the finished product were tested.

[0073] (5) The obtained precipitated fiber product and short-cut fiber were mixed at a pressure of 28 g / m 2After papermaking, hot pressing is performed to test the air permeability, tensile strength and electrical strength of the paper sample.

[0074] Comparative Example 4:

[0075] (1) Metaphenylenediamine and isophthaloyl chloride are polymerized in DMAC, and the inherent viscosity of the polymerization is controlled to be 1.6 dL / g. After neutralization and filtration, a meta-aramid resin stock solution is obtained, which is then diluted, stirred, and kept warm to obtain a meta-aramid resin solution at 40° C. with a polymer solid content of 9%.

[0076] (2) Mix water and DMAC, wherein the DMAC content is 40%, stir evenly, and cool the precipitant to 10° C. for use.

[0077] (3) The meta-aramid resin solution and the precipitating agent are injected into a high-speed rotating disc precipitator in a volume ratio of 1:12, wherein the aramid resin solution is injected through a 1.0 mm*0.1 mm spinneret hole, the distance between the nozzle and the rotor is 0.4 mm, the distance between the stator and the rotor is 0.4 mm, and the precipitator speed is 4000 rpm. The precipitate is discharged into a storage tank through the discharge port and placed overnight, and further cooled and formed to obtain a crude fiber product with a beating degree of 72°SR. The crude product is processed by cone milling, the mill power is 210 kW, the refining time is 65 min, and then after sufficient delamination and screening, a fiber slurry with a beating degree of 74°SR is obtained.

[0078] (4) The precipitated fibrillation slurry was repeatedly washed with water in a belt washer to obtain a precipitated fibrillation product with a DMAC content of 10.0 ppm. The length distribution parameters and water retention value of the finished product were tested.

[0079] (5) The obtained precipitated fiber product and short-cut fiber were mixed at a pressure of 28 g / m 2 After papermaking, hot pressing is performed to test the air permeability, tensile strength and electrical strength of the paper sample.

[0080] The length interval distribution, morphology and performance of the fibrils obtained by the above examples and comparative examples are shown in Table 1. The experimental methods and standards are as follows:

[0081] (1) The average length and distribution of the fibrids were determined by a fiber mass analyzer in accordance with ISO 16065-2 Automated optical analysis of pulp for fiber length - non-polarized light method;

[0082] (2) The water retention value of the fibrillated fiber is tested according to the determination of water retention value of pulp in GB / T 29286;

[0083] (3) The air permeability of paper is tested by using an air permeability meter according to GB / T 458-2008 Method for Determination of Air Permeability of Paper and Paperboard;

[0084] (4) The tensile strength and electrical strength of paper are tested by a tensile strength tester and a voltage tester respectively in accordance with Chapter 6 and Chapter 10 of GB / T 20629.2 Non-cellulose paper for electrical use Part 2: Test methods.

[0085] Table 1 Distribution of fiber length intervals, morphology, and performance

[0086]

[0087] It can be seen from the data of Example 1 and Comparative Example 1 in the above table that the crude fiber product is precipitated by the method of refining-fluffing-screening.

Claims

1. A method for preparing meta-aramid fiber with concentrated length distribution and high water retention value, characterized in that: The following steps are involved: (1) preparing a meta-aramid resin solution, wherein the aramid resin solution has a polymer content of 6% to 14%, a logarithmic viscosity of 1.5 to 1.8 dL / g, and a temperature of 40° C. to 70° C.; (2) injecting the meta-aramid resin solution and the precipitating agent into a precipitator through a spinneret hole, wherein the spinneret hole is rectangular, 0.5 to 5 mm long and 0.05 to 1 mm wide; the precipitator comprises a stator and a rotor, the spacing between the spinneret hole and the rotor is 0.2 to 1.0 mm, and the spacing between the stator and the rotor is 0.2 to 1.0 mm; precipitating and cooling to form a crude fiber product, the crude fiber product is subjected to pulping, delamination and sieving, the pulping is a cone mill, the pulping power is 150 to 250 kW, and the pulping time is 20 to 60 min; obtaining a precipitated fiber slurry; the beating degree of the precipitated fiber slurry is 65 to 85 o SR, weight-average length is 0.7-1.0 mm, width is greater than 23 μm, the proportion of overlong fibers is less than 1.0%, the proportion of fine fibers is less than 10%, and the water retention value is greater than 300%; (3) Washing the fiber slurry to obtain meta-aramid fiber with concentrated length distribution and high water retention value.

2. The preparation method according to claim 1, characterized in that The step (1) of preparing the meta-aramid resin solution specifically comprises: polymerizing meta-phenylenediamine and isophthaloyl chloride in an amide solvent, neutralizing and filtering to obtain a meta-aramid resin stock solution, and then diluting and stirring to obtain a meta-aramid resin solution.

3. The preparation method according to claim 1, characterized in that: The precipitating agent in step (2) is an amide solvent, the mass content is 25% to 50%, and the temperature is 0°C to 30°C.

4. The preparation method according to claim 2 or 3, characterized in that: The amide solvent is N,N-dimethylformamide and / or N,N-dimethylacetamide.

5. The preparation method according to claim 1, characterized in that: In step (2), the volume ratio of the meta-aramid resin solution to the precipitating agent is 1:10-25, and the rotating speed of the precipitator is 3000-6000 rpm.

6. A meta-aramid fiber with a concentrated length distribution and high water retention value obtained by the preparation method according to any one of claims 1 to 5, characterized in that: The residual solvent content in the precipitated fibrids was less than 100 ppm.

7. The fibrid according to claim 6, characterized in that The fibrillation and short-cut fibers are paper-made and then hot-pressed to obtain meta-aramid paper.