A comprehensive process for recovering metals and non-metals from tungsten tailings
Through the fluorine-free and acid-free process flow and equipment combination, combined with slurry mixing and flotation technology, the problem of insufficient separation technology of feldspar and quartz is solved, the comprehensive recovery of metals and non-metals in tailings is achieved, and tailings emissions are reduced. Improved resource utilization and business efficiency.
Patent Information
- Application Number
- CN202111079182.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-15
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-09-15
AI Technical Summary
There are deficiencies in the separation technology of feldspar and quartz in the existing technology, which results in the failure to effectively recycle non-metallic mineral resources in metal mine tailings, resulting in resource waste and environmental pollution.
Using a fluorine-free and acid-free process, through cyclone, plate magnetic separator and spiral chute and other equipment, combined with slurry mixing and flotation technology, mica, quartz and feldspar are separated, using anion and cation associates, metal ion activation Collecting agents such as agents and anionic collectors can achieve comprehensive recovery of metals and non-metals in tailings.
It effectively reduces tailings emissions, improves resource utilization, recovers a large amount of non-metallic mineral resources, improves corporate efficiency, achieves further recovery of tungsten metal, and extends the service life of tailings ponds.
Smart Images

Figure CN115805134B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of mineral flotation, and in particular relates to a process for comprehensively recovering metals and non-metals in tungsten tailings. Background Art
[0002] my country's metal mine tailings contain a large amount of non-metallic mineral resources such as feldspar, quartz, and mica. However, most metal mining companies only focus on the secondary recovery of the target metals in the tailings. However, due to the reasons of mineral processing technology and equipment, the non-metallic mineral resources in the metal mine tailings have not been sorted and utilized. The tailings ponds accumulated in my country's metal mines have become a resource library with rich reserves of non-metallic mineral resources. The comprehensive utilization of metal mine tailings has important significance for reducing the waste of mineral resources, reducing the discharge of mine solid waste, increasing corporate benefits, and avoiding excessive exploitation of non-metallic mines.
[0003] The storage capacity of tailings ponds in my country's metal mines is decreasing day by day. Taking Ninghua Xingluokeng Tungsten Mine Co., Ltd. as an example, Wangtongkeng Tailings Pond is its supporting facility. It was built and put into operation in 2008. It is the only tailings pond currently in operation in the concentrator. The designed service life is 17 years. The total tailings storage volume is 26.7 million tons. The daily tailings volume of the concentrator is about 5,000 tons. At present, the remaining storage capacity of the tailings pond is only 20% of the designed storage capacity. The decreasing remaining storage capacity of the tailings pond has become an important factor restricting the daily production of the Xingluokeng Tungsten Mine Concentrator. Comprehensive analysis, exploring how to reduce tailings discharge in bulk and increase the service life of the tailings pond of the tungsten ore concentrator is imminent.
[0004] As an important strategic mineral resource, quartz is widely used in traditional industries such as glass, ceramics, cement, as well as high-tech fields such as aerospace, military, semiconductors, and solar energy. Feldspar is widely used in ceramics, glass, potash fertilizers, thermal insulation materials, and other fields. However, due to the technical defects of feldspar and quartz separation, most of the relevant industries in my country only mine single feldspar or quartz minerals, and the quality of the mined ore directly determines its value. At present, the research on the flotation separation of feldspar and quartz in tailings mainly adopts the "fluorine-free acid method" and the "fluorine-containing acid method". Both methods have great harm to the environment and equipment. These factors have greatly limited the comprehensive utilization of non-metallic mineral resources in tailings in actual production.
[0005] Therefore, according to the actual situation of the tailings pond of the tungsten ore concentrator, a comprehensive treatment plan for tungsten tailings is technically developed, ultimately realizing the recovery of metallic tungsten, as well as non-metallic feldspar and quartz in the tailings. Summary of the invention
[0006] The technical problem to be solved by the present invention is to overcome the deficiencies and defects of the fluorine-free and acid-free flotation separation technology of feldspar and quartz in the background technology and to solve the problem of comprehensive recovery and utilization of non-metallic minerals in tailings.
[0007] In order to solve the above technical problems, the technical solution proposed by the present invention is:
[0008] The present invention discloses a comprehensive process for recovering metals and non-metals from tungsten tailings; the tungsten tailings are taken as the processing object, and the tailings are ground to a fineness of -0.074mm, accounting for 67%-75%. A cyclone is used for desludging, and the cyclone sand is processed by a flat magnetic separator, and then a spiral chute is used for classification; the tailings of the spiral chute are the second desludging of the grinding product, and the concentrate of the spiral chute is used to recover metal tungsten. The ore in the spiral chute is separated into mica, quartz and feldspar through a flotation process; specifically:
[0009] After slurry adjustment and controlling the pH value of the slurry to 10.00-10.60, the ore in the spiral chute is first separated from mica by flotation, and then separated from quartz by flotation at a pH value of 10.60-11.00; the residue at the bottom of the trough after the quartz flotation is the feldspar product; the collector type for mica flotation separation is an anion-cation complex collector; the activator type for quartz flotation separation is a metal ion activator, the collector type is an anion collector, and the collector for quartz acid separation is a cationic collector.
[0010] As a preferred solution, the present invention provides a process for comprehensively recovering metals and non-metals in tungsten tailings; after the spiral chute concentrate is treated by three shaking tables, the slurry is adjusted and sulfide flotation is performed to remove impurities, and the flotation tailings are tungsten concentrate.
[0011] As a preferred solution, the present invention provides a process for comprehensive recovery of metals and non-metals in tungsten tailings. The ore in the spiral chute is separated into mica, quartz and feldspar through flotation process. Mica is first separated by flotation under the condition of pulp pH of 10.00-10.60, and then quartz is separated by flotation under the condition of pH 10.60-11.00. The residue at the bottom of the tank after quartz flotation is the feldspar product. The collector type of mica flotation separation is anion-cation association collector; the activator type of quartz flotation separation is metal ion activator, and the collector type is anion collector.
[0012] As a preferred embodiment, the present invention provides a process for comprehensive recovery of metals and non-metals in tungsten tailings; the anionic collectors are all fatty acid collectors: at least one of oleic acid, oxidized paraffin soap, and tall oil; the cationic collectors are all amine collectors: at least one of dodecylamine, octadecylamine, and etheramine.
[0013] As a preferred embodiment, the present invention provides a process for comprehensively recovering metals and non-metals in tungsten tailings; the anion-cation complex collector for mica flotation is composed of anion collector and cationic collector in a mass ratio; wherein the anion collector: cationic collector = 3:1-5:1.
[0014] As a preferred embodiment, the present invention provides a process for comprehensively recovering metals and non-metals in tungsten tailings; the activator for quartz flotation is calcium ions, preferably calcium chloride reagent.
[0015] As a preferred embodiment, the present invention provides a process for comprehensive recovery of metals and non-metals in tungsten tailings, comprising the following steps:
[0016] The first step is to add sodium carbonate to the tailings according to the standard of adding 1000-1500g of sodium carbonate per ton of tailings for grinding, so that the fineness of the grinding product reaches -0.074mm and the content is 65-75%;
[0017] In the second step, the feed of the hydrocyclone is the grinding product, the feed concentration is 30-35%, and the feed pressure is 0.15MPa; the feed of the flat magnetic separator is the hydrocyclone sand settling, the feed concentration is 25-30%, the magnetic field strength is 7000-8000Gs, and the non-magnetic product is washed with a concentration of 20-25%, and is directly graded in the spiral chute;
[0018] In the third step, after the concentrate in the spiral chute is processed by three shaking tables, 50-70g of xanthate and 15-25g of No. 2 oil are added to each ton of shaker concentrate to flotate and remove impurities. The flotation tailings are tungsten concentrate. According to the current price of tungsten concentrate and the daily output of 3,000 tons of tailings, the tungsten concentrate recovered from the tailings will generate an additional profit of about 7.5 million yuan;
[0019] In the fourth step, sodium carbonate is added to the middlings in the spiral chute to adjust the pH value of the pulp to 10.00-10.60, and 300-400g / t of anion-cation complex collector is added per ton of tailings to float and separate mica from the tailings. The pulp is continued to be adjusted to 10.00-10.60, and the dosage of the reagent is halved for one sweep;
[0020] Step 6: Add sodium carbonate to adjust the pH value of the slurry to 10.60-11.00, add 150-250g of Ca ions and 300-500g of anion collector per ton of tailings to float and separate the quartz in the tailings, continue to adjust the slurry to 10.60-11.00, and reduce the dosage of reagents by half to scavenging; after scavenging and / or flotation of quartz, the material remaining at the bottom of the tank is mainly feldspar, and the feldspar is subjected to high gradient iron removal, the magnetic field strength is 1.5-1.8T, and the non-magnetic product is high-quality feldspar;
[0021] Step 7: The foam product (i.e., quartz product) is slurried, the pH of the slurry is adjusted to 10.60-11.00, the slurry concentration is 25-35%, and the ore is concentrated twice without adding chemicals. The tailings of each concentration operation are returned to the previous operation in sequence;
[0022] In the eighth step, the foam product (i.e., quartz product) that has been selected twice is re-slurried, the pH value of the slurry is adjusted to 2.70-3.20, 60-80g of cationic collector is added per ton of tailings, and quartz is removed by aeration. The slurry is continued to be adjusted to 2.70-3.20, and the dosage of the reagent is halved for one sweep; after two flotation separations, the main substance remaining at the bottom of the tank is high-quality quartz.
[0023] As a preferred solution, the present invention provides a process for comprehensively recovering metals and non-metals in tungsten tailings; the silicon dioxide content in the obtained quartz product is greater than or equal to 99.2%; the potassium oxide and sodium oxide contents in the obtained high-quality feldspar product will vary with the properties of the original ore, but both meet the first-class product standards.
[0024] As one of the preferred solutions, the present invention provides a process for comprehensively recovering metals and non-metals from tungsten tailings, comprising the following steps:
[0025] Pre-processing
[0026] Sodium carbonate is added to the tailings according to the standard of adding 1200g of sodium carbonate per ton of tailings for grinding, so that the fineness of the grinding product reaches -0.074mm and the content is 67.5%, and the ground tailings are mixed with water to form a 33.5% slurry;
[0027] Cyclone desludging
[0028] The prepared slurry is pumped to the hydrocyclone for desiccation, and the feed pressure is 0.15MPa; the overflow product and the sedimentation product are obtained;
[0029] Spiral chute classification
[0030] The feed of the flat plate magnetic separator is cyclone sand settling, the feed concentration is 27%, the magnetic field strength is 7500Gs, the non-magnetic product is adjusted to 22% and transported to the spiral chute for classification. The spiral chute concentrate is the selected ore of metal tungsten; the middling ore is the ore separated by flotation of feldspar and quartz; the tailings is the removed fine mud.
[0031] After the concentrate from the spiral chute is treated by three shaking tables, 57g of xanthate and 20g of No. 2 oil are added per ton of shaker concentrate to flotate and remove impurities from the tungsten concentrate. The flotation tailings are tungsten concentrate with a grade of 55.3% and a yield of 0.0081%.
[0032] The spiral chute is used for flotation separation of feldspar and quartz. The specific process is as follows:
[0033] Mica flotation: sodium carbonate was added to adjust the pH value of the pulp to 10.40, the mass ratio of anion and cation associated collectors was fixed to 3:1, wherein the anion collector was sodium oleate; the cationic collector was dodecylamine, the total dosage of mica roughing agent was 350g / t, the pulp was continued to be adjusted to 10.40, the dosage of the agent was halved and the first sweep was performed, the yield of the foam product, i.e. the mica product, was 11.59%, and the bottom product was subjected to quartz and feldspar flotation separation;
[0034] Quartz flotation
[0035] Sodium carbonate was added to adjust the pH value of the ore pulp to 10.75, and 180g of Ca ions and 360g of anionic collector-sodium oleate were added per ton of tailings to separate the quartz in the tailings by flotation; sodium carbonate was continued to be added to adjust the pH value of the ore pulp to 10.75, and the dosage of the reagent was halved to sweep the first layer, and the bottom of the flotation tank was the feldspar product;
[0036] Quartz Selection
[0037] The quartz product is enriched in the flotation foam. The froth product of quartz flotation is pulped, and sodium carbonate is added to adjust the pH value of the pulp to 10.75. The first stage of selection is carried out without adding chemicals. The bottom of the flotation tank is the medium ore, which is returned to the quartz scavenging operation. The foam of the first stage of quartz selection is pulped, and sodium carbonate is added to adjust the pH value of the pulp to 10.75. The second stage of selection is carried out without adding chemicals. The bottom of the flotation tank is the medium ore, which is returned to the first stage of quartz selection operation.
[0038] Quartz weak acid impurity removal
[0039] The foam product after two flotation selections is slurried to a pH of 2.75. 70g of cationic collector dodecylamine is added per ton of tailings, and quartz is removed by aeration. The slurry is then adjusted to 2.75 and the dosage of reagents is halved to remove impurities. After two flotation selections, quartz is mainly left at the bottom of the tank.
[0040] As one of the preferred solutions, the present invention provides a process for comprehensively recovering metals and non-metals from tungsten tailings, comprising the following steps:
[0041] Pre-processing
[0042] Add sodium carbonate to the tailings according to the standard of adding 1400g sodium carbonate per ton of tailings for grinding, so that the fineness of the grinding product reaches -0.074mm and the content is 66.1%, and the ground tailings are mixed with water to form a 35% slurry;
[0043] Cyclone desludging
[0044] The prepared slurry is pumped to the hydrocyclone for desiccation, and the feed pressure is 0.15MPa; the overflow product and the sedimentation product are obtained;
[0045] Spiral chute classification
[0046] The feed of the flat plate magnetic separator is cyclone sedimentation, the feed concentration is 28%, the magnetic field strength is 7500Gs, the non-magnetic product is adjusted to 24% and transported to the spiral chute for classification. The spiral chute concentrate is the selected ore of metal tungsten; the middling ore is the ore separated by flotation of feldspar and quartz; the tailings is the removed fine mud;
[0047] After the concentrate from the spiral chute is processed by three shaking tables, 65g of xanthate and 23g of No. 2 oil are added per ton of shaker concentrate to flotate and remove impurities from the tungsten concentrate. The flotation tailings are tungsten concentrate with a grade of 55.6% and a yield of 0.0087%.
[0048] The spiral chute is used for flotation separation of feldspar and quartz. The specific process is as follows:
[0049] Mica flotation: sodium carbonate was added to adjust the pH value of the pulp to 10.38, the mass ratio of anion and cation associated collectors was fixed at 5:1, wherein the anion collector was tall oil; the cationic collector was etheramine, the total dosage of mica roughing agent was 400g / t, the pulp was continued to be adjusted to 10.38, the dosage of the agent was halved, and the yield of the foam product, i.e. the mica product, was 12.93%, and the bottom product was subjected to quartz and feldspar flotation separation;
[0050] Quartz flotation: add sodium carbonate to adjust the pH value of the pulp to 10.95, add 220g of Ca ions and 440g of anionic collector-oxidized paraffin soap per ton of tailings, and flotation separate the quartz in the tailings; continue to add sodium carbonate to adjust the pH value of the pulp to 10.95, reduce the dosage of reagents by half, and sweep the first layer. The bottom of the flotation tank is feldspar products.
[0051] Quartz selection: Quartz products are enriched in flotation foam. The foam products of quartz flotation are pulped, sodium carbonate is added to adjust the pH value of the pulp to 10.95, and the first selection is carried out without adding chemicals. The bottom of the flotation tank is the medium ore, which is returned to the quartz sweeping operation; the foam of the first selection of quartz is pulped, sodium carbonate is added to adjust the pH value of the pulp to 10.95, and the second selection is carried out without adding chemicals. The bottom of the flotation tank is the medium ore, which is returned to the first selection of quartz;
[0052] Quartz weak acid impurity removal: the foam product after two flotation selections is slurried to a pH of 3.00. 65g of cationic collector etheramine is added per ton of tailings, and quartz impurities are removed by aeration. The slurry is continued to be adjusted to 3.00, and the dosage of reagents is halved for one sweep. After two flotation selections, the main substance remaining at the bottom of the tank is quartz.
[0053] Compared with the prior art, the advantages of the present invention are:
[0054] (1) The process of the present invention is carried out under fluorine-free and acid-free slurry conditions, which not only recovers a large amount of non-metallic mineral resources, but also can greatly reduce the discharge of mine tailings. The mica obtained by the present invention can also be used in the insulation board industry. After the treatment of the present invention, the discharge of tailings can be reduced to less than 15wt%. This resource utilization rate is much higher than the existing technology.
[0055] (2) The present invention not only recovers non-metallic materials, but also further recovers metallic tungsten in the tailings, greatly improving the efficiency of the enterprise. At the same time, most of the equipment used in the present invention is existing tungsten ore processing equipment, and the maximum recovery of resources is achieved through the reasonable docking of each process and the optimization of the process parameters of each process. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Figure 1 This is the XRD diagram of the tungsten tailings from the Xingluokeng concentrator;
[0057] Figure 2 This is the XRD pattern of fine mud in the process;
[0058] Figure 3 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0059] The technical solution of the present invention is further described in detail below through specific implementation methods.
[0060] The following examples and comparative examples are based on the technology development exploration of the gravity separation tailings of Ninghua Xingluokeng tungsten mine as raw materials. The main phase analysis of the gravity separation tailings of tungsten is shown in Figure 1 The contents of the main substances are shown in Table 1. The mineral composition of the gravity-selected tailings is mainly quartz, feldspar, mica and some impurities with less content. The tailings fineness -0.074mm accounts for 12.73%, the relative content of mica minerals is about 14%, the relative content of quartz minerals is about 48%, and the relative content of feldspar minerals is about 33%. The content of the three minerals in the gravity-selected tailings is about 95%.
[0061] Table 1. Properties of gravity separation tailings from Xingluokeng tungsten mine
[0062]
[0063] Example 1
[0064] This embodiment uses the process technology provided by the present invention to separate mica, quartz and feldspar from the re-selection tailings of tungsten in Ninghua, Fujian, so that the feldspar product reaches the first-class quality and the quartz product reaches the sales standard.
[0065] The present embodiment provides a flotation separation process for flotation separation of mica and quartz feldspar from tailings, which specifically includes the following steps:
[0066] Pre-treatment (grinding, desludging): add 1200g of sodium carbonate per ton of tailings to the tailings for grinding, so that the fineness of the ground product reaches -0.074mm and the content is 67.5%, and the ground tailings are mixed with water to form a 33.5% slurry.
[0067] Hydrocyclone desludging: The slurry is pumped to the hydrocyclone for desludging, and the feed pressure is 0.15 MPa. The particle size screening results of the overflow product and the sedimentation product are shown in Table 2.
[0068] Spiral chute classification: The feed of the flat magnetic separator is cyclone sand settling, the feed concentration is 27%, the magnetic field strength is 7500Gs, the non-magnetic product is slurried down to 22%, and transported to the spiral chute for classification. The spiral chute concentrate is the selected ore of metal tungsten; the middling ore is the ore separated by flotation of feldspar and quartz; the tailings is the removed fine mud, and its particle size screening results are shown in Table 2.
[0069] Table 2. Screening results of cyclone, flat magnetic separator and spiral chute products
[0070]
[0071] The tailings from the cyclone overflow and spiral chute are fine in size. The phase analysis diagram is as shown in the attached manual. Figure 2 As shown, its main components are quartz, feldspar, mica and a very small amount of silicate minerals, which can be used as high-quality raw materials for cement and ceramic bodies.
[0072] After the concentrate in the spiral chute is treated by three shaking tables, 57g of xanthate and 20g of No. 2 oil are added to each ton of shaking table concentrate for tungsten concentrate flotation and impurity removal. The flotation tailings are tungsten concentrate with a grade of 55.3% and a yield of 0.0081%. According to the current price of tungsten concentrate and the daily output of 3,000 tons of tailings, the tungsten concentrate recovered from the tailings has an additional profit of approximately RMB 7.5 million.
[0073] The spiral chute is used for flotation separation of feldspar and quartz. The specific process is as follows:
[0074] Mica flotation: sodium carbonate was added to adjust the pH value of the pulp to 10.40, the ratio (mass ratio) of anion and cation associated collectors was fixed at 3:1 (among which the anion collector was sodium oleate and the cationic collector was dodecylamine), the total dosage of mica roughing agent was 350g / t, the pulp was continued to be adjusted to 10.40, the dosage of the agent was halved for one sweep, the yield of the foam product (i.e. mica product) was 11.59%, and the bottom product was separated by quartz and feldspar by flotation.
[0075] Quartz flotation: sodium carbonate was added to adjust the pH value of the pulp to 10.75, 180g of Ca ions and 360g of anionic collector-sodium oleate were added per ton of tailings, and quartz in the tailings was separated by flotation; sodium carbonate was continued to be added to adjust the pH value of the pulp to 10.75, and the dosage of the reagent was halved to sweep the first layer. The bottom of the flotation tank was the feldspar product, which was subjected to high gradient iron removal. The non-magnetic product was filtered and dried for testing. The test results are shown in Table 3.
[0076] Quartz selection: Quartz products are mainly enriched in flotation foam. The foam product of quartz flotation is pulped, sodium carbonate is added to adjust the pH value of the pulp to 10.75, and the first selection is carried out without adding chemicals. The bottom of the flotation tank is the medium ore, which is returned to the quartz sweeping operation; the foam of the first selection of quartz is pulped, sodium carbonate is added to adjust the pH value of the pulp to 10.75, and the second selection is carried out without adding chemicals. The bottom of the flotation tank is the medium ore, which is returned to the first selection of quartz;
[0077] Quartz weak acid impurity removal: The foam product after two rounds of flotation is slurried, the pulp pH is 2.75, 70g of cationic collector dodecylamine is added per ton of tailings, and the quartz impurities are removed by aeration. The pulp is continued to be adjusted to 2.75, and the dosage of the reagent is halved to sweep the first round; after two rounds of flotation impurity removal, the main residue at the bottom of the tank is high-quality quartz, which is filtered and dried for testing. The test results are shown in Table 3.
[0078] Table 3. Comparison of production indicators of feldspar products and quartz products
[0079]
[0080] It can be seen from Example 1 that through the comprehensive tailings recovery process, 23.34% of fine mud can be recovered for ceramic bodies, cement, etc., 11.59% of mica can be used in the insulation board industry, 29.57% of high-quality quartz products and 20.72% of feldspar products.
[0081] Example 2
[0082] This embodiment utilizes the process technology provided by the present invention to separate mica, quartz and feldspar from the gravity separation tailings of tungsten selection at the Xingluokeng tungsten mine, thereby making the feldspar product reach the first-class quality and the quartz product reach the sales standard.
[0083] The present embodiment provides a flotation separation process for flotation separation of mica and quartz feldspar from tailings, which specifically includes the following steps:
[0084] Pre-treatment (grinding, desludging): add 1300g of sodium carbonate per ton of tailings to the tailings for grinding, so that the fineness of the ground product reaches -0.074mm and the content is 68.8%. The ground tailings are mixed with water to form a 33.5% slurry.
[0085] Hydrocyclone desludging: The slurry is pumped to the hydrocyclone for desludging, and the feed pressure is 0.15 MPa. The particle size screening results of the overflow product and the sedimentation product are shown in Table 4.
[0086] Spiral chute classification: The feed of the flat magnetic separator is cyclone sand settling, the feed concentration is 25%, the magnetic field strength is 7500Gs, the non-magnetic product is slurried down to 23%, and then transported to the spiral chute for classification. The spiral chute concentrate is the selected ore of metal tungsten; the middling ore is the ore separated by flotation of feldspar and quartz; the tailings is the removed fine mud, and the particle size screening results are shown in Table 2.
[0087] Table 4. Screening results of cyclone, flat magnetic separator and spiral chute products
[0088]
[0089] The tailings from the cyclone overflow and spiral chute are fine in size. The phase analysis diagram is as shown in the attached manual. Figure 2 As shown, its main components are quartz, feldspar, mica and a very small amount of silicate minerals, which can be used as high-quality raw materials for cement and ceramic bodies.
[0090] After the concentrate in the spiral chute is treated by three shaking tables, 60g of xanthate and 22g of No. 2 oil are added to each ton of shaking table concentrate for tungsten concentrate flotation and impurity removal. The flotation tailings are tungsten concentrate with a grade of 55.8% and a yield of 0.0084%. According to the current price of tungsten concentrate and the daily output of 3,000 tons of tailings, the tungsten concentrate recovered from the tailings has an additional profit of approximately RMB 7.5 million.
[0091] The spiral chute is used for flotation separation of feldspar and quartz. The specific process is as follows:
[0092] Mica flotation: sodium carbonate was added to adjust the pH value of the pulp to 10.50, the ratio (mass ratio) of anion and cation associated collectors was fixed at 4:1 (the anion collector was oxidized paraffin soap; the cationic collector was octadecylamine), the total dosage of mica roughing agent was 380g / t, the pulp was continued to be adjusted to 10.50, the dosage of the agent was halved for sweeping, the yield of the foam product (i.e. mica product) was 12.47%, and the bottom product was separated by quartz and feldspar by flotation.
[0093] Quartz flotation: sodium carbonate was added to adjust the pH value of the pulp to 10.85, and 200g of Ca ions and 400g of anionic collector-oxidized paraffin soap were added per ton of tailings to separate the quartz in the tailings by flotation; sodium carbonate was continued to be added to adjust the pH value of the pulp to 10.85, and the dosage of the reagent was halved to sweep the first layer. The feldspar product was at the bottom of the flotation tank, and high gradient iron removal was carried out. The non-magnetic product was filtered and dried for testing. The test results are shown in Table 5.
[0094] Quartz selection: Quartz products are mainly enriched in flotation foam. The foam product of quartz flotation is pulped, sodium carbonate is added to adjust the pH value of the pulp to 10.85, and the first selection is carried out without adding chemicals. The bottom of the flotation tank is the medium ore, which is returned to the quartz sweeping operation; the foam of the first selection of quartz is pulped, sodium carbonate is added to adjust the pH value of the pulp to 10.85, and the second selection is carried out without adding chemicals. The bottom of the flotation tank is the medium ore, which is returned to the first selection of quartz;
[0095] Quartz weak acid impurity removal: The foam product after two rounds of flotation is slurried, the pulp pH is 2.90, 75g of cationic collector octadecylamine is added per ton of tailings, and the quartz impurities are removed by aeration. The pulp is continued to be adjusted to 2.90, and the dosage of the reagent is halved to sweep the first round; after two rounds of flotation impurity removal, the main residue at the bottom of the tank is high-quality quartz, which is filtered and dried for testing. The test results are shown in Table 3.
[0096] Table 5. Comparison of production indicators of feldspar products and quartz products
[0097]
[0098] It can be seen from Example 2 that through the comprehensive tailings recovery process, 24.62% of fine mud can be recovered for ceramic bodies, cement, etc., 12.47% of mica can be used in the insulation board industry, 29.21% of high-quality quartz products and 19.82% of feldspar products.
[0099] Example 3
[0100] This embodiment utilizes the process technology provided by the present invention to separate mica, quartz and feldspar from the gravity separation tailings of tungsten selection at the Xingluokeng tungsten mine, thereby making the feldspar product reach the first-class quality and the quartz product reach the sales standard.
[0101] The present embodiment provides a flotation separation process for flotation separation of mica and quartz feldspar from tailings, which specifically includes the following steps:
[0102] Pre-treatment (grinding, desludging): add 1400g of sodium carbonate per ton of tailings to the tailings for grinding, so that the fineness of the ground product reaches -0.074mm and the content is 66.1%. The ground tailings are mixed with water to form a 35% slurry.
[0103] Hydrocyclone desludging: The slurry is pumped to the hydrocyclone for desludging, and the feed pressure is 0.15 MPa. The particle size screening results of the overflow product and the sedimentation product are shown in Table 4.
[0104] Spiral chute classification: The feed of the flat magnetic separator is cyclone sand settling, the feed concentration is 28%, the magnetic field strength is 7500Gs, the non-magnetic product is slurried down to 24%, and transported to the spiral chute for classification. The spiral chute concentrate is the selected ore of metal tungsten; the middling ore is the ore separated by flotation of feldspar and quartz; the tailings is the removed fine mud, and its particle size screening results are shown in Table 2.
[0105] Table 4. Screening results of cyclone, flat magnetic separator and spiral chute products
[0106]
[0107] The tailings from the cyclone overflow and spiral chute are fine in size. The phase analysis diagram is as shown in the attached manual. Figure 2 As shown, its main components are quartz, feldspar, mica and a very small amount of silicate minerals, which can be used as high-quality raw materials for cement and ceramic bodies.
[0108] After the concentrate in the spiral chute is treated by three shaking tables, 65g of xanthate and 23g of No. 2 oil are added to each ton of shaking table concentrate for tungsten concentrate flotation and impurity removal. The flotation tailings are tungsten concentrate with a grade of 55.6% and a yield of 0.0087%. According to the current price of tungsten concentrate and the daily output of 3,000 tons of tailings, the tungsten concentrate recovered from the tailings has an additional profit of approximately RMB 7.5 million.
[0109] The spiral chute is used for flotation separation of feldspar and quartz. The specific process is as follows:
[0110] Mica flotation: sodium carbonate was added to adjust the pH value of the pulp to 10.38, the ratio (mass ratio) of anion and cation associated collectors was fixed at 5:1 (the anion collector was tall oil and the cationic collector was ether amine), the total dosage of mica roughing agent was 400g / t, the pulp was continued to be adjusted to 10.38, the dosage of the agent was halved and swept, the yield of the foam product (i.e. mica product) was 12.93%, and the bottom product was separated by quartz and feldspar by flotation.
[0111] Quartz flotation: sodium carbonate was added to adjust the pH value of the pulp to 10.95, 220g of Ca ions and 440g of anionic collector-oxidized paraffin soap were added per ton of tailings, and quartz in the tailings was separated by flotation; sodium carbonate was continued to be added to adjust the pH value of the pulp to 10.95, and the dosage of the reagent was halved to sweep the first layer. The feldspar product was at the bottom of the flotation tank, and high gradient iron removal was carried out. The non-magnetic product was filtered and dried for testing. The test results are shown in Table 5.
[0112] Quartz selection: Quartz products are mainly concentrated in flotation foam. The foam product of quartz flotation is pulped, sodium carbonate is added to adjust the pH value of the pulp to 10.95, and the first selection is carried out without adding chemicals. The bottom of the flotation tank is the medium ore, which is returned to the quartz scavenging operation; the foam of the first selection of quartz is pulped, sodium carbonate is added to adjust the pH value of the pulp to 10.95, and the second selection is carried out without adding chemicals. The bottom of the flotation tank is the medium ore, which is returned to the first selection of quartz;
[0113] Quartz weak acid impurity removal: The foam product after two rounds of flotation is slurried, the pulp pH is 3.00, 65g of cationic collector etheramine is added per ton of tailings, and the quartz impurities are removed by aeration. The pulp is continued to be adjusted to 3.00, and the dosage of the reagent is halved to sweep the first round; after two rounds of flotation impurity removal, the main residue at the bottom of the tank is high-quality quartz, which is filtered and dried for testing. The test results are shown in Table 6.
[0114] Table 6. Comparison of production indicators of feldspar products and quartz products
[0115]
[0116] It can be seen from Example 3 that through the comprehensive tailings recovery process, 23.66% of fine mud can be recovered for ceramic bodies, cement, etc., 12.93% of mica can be used in the insulation board industry, 30.34% of high-quality quartz products and 22.58% of feldspar products.
[0117] Comparative Example 1
[0118] Other conditions are the same as those in Example 1, except that:
[0119] Hydrocyclone desludging: The ground tailings are mixed with water to form a 40% slurry, and the prepared slurry is pumped to the hydrocyclone for desludging, with a feed pressure of 0.15 MPa. The particle size screening results of the overflow product and the sedimentation product are shown in Table 7.
[0120] Spiral chute classification: The feed of the flat magnetic separator is cyclone sand settling, the feed concentration is 35%, the magnetic field strength is 7500Gs, the non-magnetic product is slurried down to 30%, and transported to the spiral chute for classification. The spiral chute concentrate is the selected ore of metal tungsten; the middling ore is the ore separated by flotation of feldspar and quartz; the tailings is the removed fine mud, and its particle size screening results are shown in Table 7.
[0121] Table 7. Screening results of cyclone, flat magnetic separator and spiral chute products
[0122]
[0123] From the comparative example, we can see that: when the feed concentration of the cyclone increases, the overflow product has a significantly coarser particle size; when the feed concentration of the flat magnetic separator increases, the entrainment of magnetic products increases significantly; when the feed concentration of the spiral chute increases, the particle size distribution of the tailings also becomes significantly coarser.
[0124] This leads to
[0125] Comparative Example 2 and Comparative Example 3
[0126] Other conditions are the same as those in Example 2, except that:
[0127] The spiral chute is used for flotation separation of feldspar and quartz. The specific process is as follows:
[0128] Quartz flotation: Sodium carbonate was added to adjust the pH values of the ore pulps of Comparative Example 2 and Comparative Example 3 to 10.00 and 12.00, respectively. 200g of Ca ions and 400g of anionic collector-oxidized paraffin soap were added per ton of tailings to separate the quartz in the tailings by flotation; Sodium carbonate was continued to be added to adjust the pH values of the ore pulps of Comparative Example 2 and Comparative Example 3 to 10.00, and the dosage of the reagent was halved to sweep the selection. The feldspar product was at the bottom of the flotation tank, and high gradient iron removal was carried out. The non-magnetic product was filtered and dried for testing. The test results are shown in Table 8.
[0129] Quartz selection: Quartz products are mainly enriched in flotation foam. The foam product of quartz flotation is slurried, and sodium carbonate is added to adjust the pH value of the slurry of Comparative Example 2 and Comparative Example 3 to 10.00 and 12.00 respectively. The first selection is performed without adding chemicals. The bottom of the flotation tank is medium ore, which is returned to the quartz scavenging operation; The foam of the first selection of quartz is slurried, and sodium carbonate is added to adjust the pH value of the slurry of Comparative Example 2 and Comparative Example 3 to 10.00 and 12.00 respectively. The second selection is performed without adding chemicals. The bottom of the flotation tank is medium ore, which is returned to the first selection of quartz;
[0130] Quartz weak acid impurity removal: The foam product after two rounds of flotation is slurried, the pulp pH is 2.90, 75g of cationic collector octadecylamine is added per ton of tailings, and the quartz impurities are removed by aeration. The pulp is continued to be adjusted to 2.90, and the dosage of the reagent is halved to sweep the first round; after two rounds of flotation impurity removal, the main residue at the bottom of the tank is high-quality quartz, which is filtered and dried for testing. The test results are shown in Table 8.
[0131] Table 8. Comparison of production indicators of feldspar products and quartz products
[0132]
[0133]
[0134] Comparative Examples 2 and 3 show that when the pH value of feldspar and quartz separation is too low, the yield of quartz product is low, and the feldspar product index is not suitable. When the pH value of feldspar and quartz separation is too high, the feldspar yield is low, and the quartz product index is unqualified.
[0135] Comparative Example 4 and Comparative Example 5
[0136] Other conditions are the same as those in Example 3, except that:
[0137] The spiral chute is used for flotation separation of feldspar and quartz. The specific process is as follows:
[0138] Quartz flotation: Sodium carbonate was added to adjust the pH value of the ore pulp of Comparative Examples 4 and 5 to 10.95. In Comparative Example 4, 300 g of Ca ions and 400 g of anionic collector-oxidized paraffin soap were added per ton of tailings to separate the quartz in the tailings by flotation; in Comparative Example 5, 200 g of Ca ions and 600 g of anionic collector-oxidized paraffin soap were added per ton of tailings to separate the quartz in the tailings by flotation. Sodium carbonate was continued to be added to adjust the pH value of the ore pulp of Comparative Examples 4 and 5 to 10.95, and the dosage of the reagent was halved to sweep one layer. The bottom of the flotation tank was a feldspar product, and high gradient iron removal was carried out. The non-magnetic product was filtered and dried for testing. The test results are shown in Table 9.
[0139] Quartz selection: Quartz products are mainly enriched in flotation foam. The foam product of quartz flotation is slurried, sodium carbonate is added to adjust the pH value of the slurry of Comparative Example 4 and Comparative Example 5 to 10.95, and the first selection is performed without adding chemicals. The bottom of the flotation tank is medium ore, which is returned to the quartz scavenging operation; the foam of the first selection of quartz is slurried, sodium carbonate is added to adjust the pH value of the slurry of Comparative Example 4 and Comparative Example 5 to 10.95, and the second selection is performed without adding chemicals. The bottom of the flotation tank is medium ore, which is returned to the first selection of quartz;
[0140] Quartz weak acid impurity removal: The foam product after two rounds of flotation is slurried, the pulp pH is 2.90, 75g of cationic collector octadecylamine is added per ton of tailings, and the quartz impurities are removed by aeration. The pulp is continued to be adjusted to 2.90, and the dosage of the reagent is halved to sweep the first round; after two rounds of flotation impurity removal, the main residue at the bottom of the tank is high-quality quartz, which is filtered and dried for testing. The test results are shown in Table 9.
[0141] Table 9. Comparison of production indicators of feldspar products and quartz products
[0142]
[0143] It can be seen from Comparative Examples 4 and 5 that as the dosage of the activator and the collector increases, the yield of the feldspar product is low, and the indicators of the quartz product are unqualified.
Claims
1. A process for comprehensive recovery of metals and non-metals from tungsten tailings, characterized by: Taking tungsten tailings as the treatment object, the tailings are ground to a fineness of -0.074mm, accounting for 67%-75%; a cyclone is used for desludging, and the cyclone sand is processed by a flat magnetic separator and then classified by a spiral chute; the tailings of the spiral chute are the second desludging of the grinding product, and the concentrate of the spiral chute is used to recover metal tungsten. The middlings in the spiral chute are separated from mica, quartz and feldspar through flotation process; specifically: After the ore in the spiral chute is slurried and the pH of the slurry is controlled to be 10.00-10.60, mica is first separated by flotation, and then quartz is separated by flotation at a pH of 10.60-11.00; the residue at the bottom of the trough after the quartz flotation is the feldspar product; the collector type for mica flotation separation is an anion-cation association collector; the activator for quartz flotation separation is calcium ion, the collector type is an anion collector, and the collector for quartz acid separation is a cationic collector; The spiral chute concentrate is processed by three shaking tables, and then slurry is adjusted for sulfide flotation to remove impurities, and the flotation tailings are tungsten concentrate; The anionic collectors are all fatty acid collectors, and the fatty acid collectors are selected from at least one of oleic acid, oxidized paraffin soap, and tall oil; the cationic collectors are all amine collectors, and the amine collectors are selected from at least one of dodecylamine, octadecylamine, and etheramine; The anion-cation complex collector for mica flotation is composed of anion collector and cationic collector in a mass ratio; wherein the mass ratio of anion collector to cationic collector is 3:1-5:
1.
2. A process for comprehensive recovery of metals and non-metals in tungsten tailings according to claim 1, characterized in that: The activator for quartz flotation is calcium chloride reagent.
3. A process for comprehensive recovery of metals and non-metals in tungsten tailings according to any one of claims 1-2, characterized in that: The steps include: The first step is to add sodium carbonate to the tailings according to the standard of adding 1000-1500g sodium carbonate per ton of tailings for grinding, so that the fineness of the grinding product reaches -0.074mm and the content is 65-75%, and the ground tailings are mixed with water to form a 30%-35% slurry; In the second step, the feed concentration of the cyclone is 30-35%, and the feed pressure is 0.15MPa; the magnetic field strength of the flat magnetic separator is 7000-8000Gs. After washing, the non-magnetic product has a concentration of 20-25%, and is directly graded in the spiral chute; In the third step, after the concentrate in the spiral chute is treated by three shaking tables, 50-70g of xanthate and 15-25g of No. 2 oil are added per ton of shaking table concentrate to carry out flotation and impurity removal of tungsten concentrate, and the flotation tailings are tungsten concentrate; In the fourth step, sodium carbonate is added to the middlings in the spiral chute to adjust the pH value of the pulp to 10.00-10.60, and 300-400g / t of anion-cation complex collector is added per ton of tailings to float and separate mica from the tailings. The pulp is continued to be adjusted to 10.00-10.60, and the dosage of the reagent is halved for one sweep; Step 6: Add sodium carbonate to adjust the pH value of the slurry to 10.60-11.00, add 150-250g of Ca ions and 300-500g of anion collector per ton of tailings to float and separate quartz in the tailings, continue to adjust the slurry to 10.60-11.00, and reduce the dosage of reagents by half to scavenging; after scavenging and / or flotation of quartz, the material remaining at the bottom of the tank is mainly feldspar, and the feldspar is subjected to high gradient iron removal, the magnetic field strength is 1.5-1.8T, and the non-magnetic product is feldspar; Step 7: The foam product is slurried, the pH of the slurry is adjusted to 10.60-11.00, the slurry concentration is 25-35%, and the ore is concentrated twice without adding chemicals. The tailings of each concentration operation are returned to the previous operation in sequence; In the eighth step, the foam product after two rounds of selection is re-slurried, the pH value of the slurry is adjusted to 2.70-3.20, 60-80g of cationic collector is added per ton of tailings, and quartz is removed by aeration. The slurry is continued to be adjusted to 2.70-3.20, and the dosage of reagents is halved for one round of flotation. After two rounds of flotation and impurity removal, the main substance remaining at the bottom of the tank is quartz.
4. A process for comprehensive recovery of metals and non-metals in tungsten tailings according to any one of claims 1-2, characterized in that: The silicon dioxide content in the obtained quartz product is greater than or equal to 99.2%; the potassium oxide and sodium oxide contents in the obtained high-quality feldspar product will vary with the properties of the original ore, but both meet the first-class product standards.
5. A process for comprehensive recovery of metals and non-metals in tungsten tailings according to any one of claims 1-2, characterized in that: The steps include: Pre-processing Sodium carbonate is added to the tailings according to the standard of adding 1200g of sodium carbonate per ton of tailings for grinding, so that the fineness of the grinding product reaches -0.074mm and the content is 67.5%, and the ground tailings are mixed with water to form a 33.5% slurry; Cyclone desludging The prepared slurry is pumped to the hydrocyclone for desiccation, and the feed pressure is 0.15MPa; the overflow product and the sedimentation product are obtained; Spiral chute classification The feed of the flat plate magnetic separator is cyclone sedimentation, the feed concentration is 27%, the magnetic field strength is 7500Gs, the non-magnetic product is adjusted to 22% and transported to the spiral chute for classification. The spiral chute concentrate is the selected ore of metal tungsten; the middling ore is the ore separated by flotation of feldspar and quartz; the tailings is the removed fine mud. After the concentrate from the spiral chute is processed by three shaking tables, 57g of xanthate and 20g of No. 2 oil are added per ton of shaker concentrate to flotate and remove impurities from the tungsten concentrate. The flotation tailings are tungsten concentrate with a grade of 55.3% and a yield of 0.0081%. The spiral chute is used for flotation separation of feldspar and quartz. The specific process is as follows: Mica flotation: sodium carbonate was added to adjust the pH value of the pulp to 10.40, the mass ratio of anion and cation associated collectors was fixed to 3:1, wherein the anion collector was sodium oleate; the cationic collector was dodecylamine, the total dosage of mica roughing agent was 350g / t, the pulp was continued to be adjusted to 10.40, the dosage of the agent was halved and the first sweep was performed, the yield of the foam product, i.e. the mica product, was 11.59%, and the bottom product was subjected to quartz and feldspar flotation separation; Quartz flotation Sodium carbonate was added to adjust the pH value of the ore pulp to 10.75, and 180g of Ca ions and 360g of anionic collector-sodium oleate were added per ton of tailings to separate the quartz in the tailings by flotation; sodium carbonate was continued to be added to adjust the pH value of the ore pulp to 10.75, and the dosage of the reagent was halved to sweep the first layer, and the bottom of the flotation tank was the feldspar product; Quartz Selection The quartz product is enriched in the flotation foam. The froth product of quartz flotation is pulped, and sodium carbonate is added to adjust the pH value of the pulp to 10.
75. The first stage of selection is carried out without adding chemicals. The bottom of the flotation tank is the medium ore, which is returned to the quartz scavenging operation. The foam of the first stage of quartz selection is pulped, and sodium carbonate is added to adjust the pH value of the pulp to 10.
75. The second stage of selection is carried out without adding chemicals. The bottom of the flotation tank is the medium ore, which is returned to the first stage of quartz selection operation. Quartz weak acid impurity removal The foam product after two flotation selections is slurried to a pH of 2.
75. 70g of cationic collector dodecylamine is added per ton of tailings, and quartz is removed by aeration. The slurry is then adjusted to 2.75 and the dosage of reagents is halved to remove impurities. After two flotation selections, quartz is mainly left at the bottom of the tank.
6. A process for comprehensive recovery of metals and non-metals in tungsten tailings according to any one of claims 1-2, characterized in that: The steps include: Pre-processing Sodium carbonate is added to the tailings according to the standard of adding 1400g of sodium carbonate per ton of tailings for grinding, so that the fineness of the grinding product reaches -0.074mm and the content is 66.1%, and the ground tailings are mixed with water to form a 35% slurry; Cyclone desludging The prepared slurry is pumped to the hydrocyclone for desiccation, and the feed pressure is 0.15MPa; the overflow product and the sedimentation product are obtained; Spiral chute classification The feed of the flat magnetic separator is cyclone sedimentation, the feed concentration is 28%, the magnetic field strength is 7500Gs, the non-magnetic product is adjusted to 24% and transported to the spiral chute for classification. The spiral chute concentrate is the selected ore of metal tungsten; the middling ore is the ore separated by flotation of feldspar and quartz; the tailings is the removed fine mud; After the concentrate from the spiral chute is processed by three shaking tables, 65g of xanthate and 23g of No. 2 oil are added per ton of shaker concentrate to flotate and remove impurities from the tungsten concentrate. The flotation tailings are tungsten concentrate with a grade of 55.6% and a yield of 0.0087%; The spiral chute is used for flotation separation of feldspar and quartz. The specific process is as follows: Mica flotation: sodium carbonate was added to adjust the pH value of the pulp to 10.38, the mass ratio of anion and cation associated collectors was fixed at 5:1, of which the anion collector was tall oil; the cationic collector was etheramine, the total dosage of mica roughing agent was 400g / t, the pulp was continued to be adjusted to 10.38, the dosage of the agent was halved, and the yield of the foam product, i.e. the mica product, was 12.93%, and the bottom product was subjected to quartz and feldspar flotation separation; Quartz flotation: add sodium carbonate to adjust the pH value of the pulp to 10.95, add 220g of Ca ions and 440g of anionic collector-oxidized paraffin soap per ton of tailings, and flotation separate the quartz in the tailings; continue to add sodium carbonate to adjust the pH value of the pulp to 10.95, reduce the dosage of reagents by half, and sweep the first layer. The bottom of the flotation tank is feldspar products. Quartz selection: Quartz products are enriched in flotation foam. The foam products of quartz flotation are pulped, sodium carbonate is added to adjust the pH value of the pulp to 10.95, and the first selection is carried out without adding chemicals. The bottom of the flotation tank is the medium ore, which is returned to the quartz sweeping operation; the foam of the first selection of quartz is pulped, sodium carbonate is added to adjust the pH value of the pulp to 10.95, and the second selection is carried out without adding chemicals. The bottom of the flotation tank is the medium ore, which is returned to the first selection of quartz; Quartz weak acid impurity removal: the foam product after two flotation selections is slurried to a pH of 3.
00. 65g of cationic collector etheramine is added per ton of tailings, and quartz impurities are removed by aeration. The slurry is continued to be adjusted to 3.00, and the dosage of reagents is halved for one sweep. After two flotation selections, the main substance remaining at the bottom of the tank is quartz.
Citation Information
Patent Citations
Beneficiation method for black and white tungsten fine deposit
CN101269352A
Process for recovering tungsten from very low grade tungstenic tailings