A method for preparing graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles

Through the method of cake-like graphene oxide soaking and hydrogen sintering reduction, platinum-cobalt nickel iron-copper high-entropy alloy nanoparticles were successfully prepared, solving the problem of size and phase composition control in the preparation of nanoscale high-entropy alloys, and realizing nanoparticles The uniform distribution and stability are suitable for a variety of high-performance materials applications.

CN115805319BActive Publication Date: 2024-11-01NORTHWEST INSTITUTE FOR NONFERROUS METAL RESEARCH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211485560.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-24
Publication Date
2024-11-01
Estimated Expiration
2042-11-24

AI Technical Summary

Technical Problem

It is difficult to effectively prepare nanoscale high-entropy alloy nanoparticles with a quaternary or above nanoparticles, and the problem of controlling the size and phase composition of high-entropy alloy nanoparticles has not been effectively solved.

Method used

The platinum, cobalt, nickel, iron and copper precursor salt solution was soaked in cake-like graphene oxide and then dried. The graphene-carried platinum, cobalt, nickel, iron and copper high-entropy alloy nanoparticles were prepared by hydrogen sintering, ensuring the uniformity of element distribution and substances. phase composition control.

Benefits of technology

The prepared graphene-backed platinum-cobalt nickel iron-copper high-entropy alloy nanoparticles have high specific surface area, multi-active sites and stability. They are suitable for catalysis, superconducting and biomaterial fields. The preparation method is simple, green and environmentally friendly, and suitable for industrialization. Production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115805319B_ABST
    Figure CN115805319B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing graphene-supported platinum-cobalt-nickel-iron-copper high entropy alloy nanoparticles, the method comprising: first, preparing a platinum-cobalt-nickel-iron-copper precursor salt solution of five elements of platinum, cobalt, nickel, iron and copper, and then putting freeze-dried cake-shaped graphene oxide into the solution for soaking; second, taking out the soaked cake-shaped graphene oxide, drying it and calcining and reducing it to obtain graphene-supported platinum-cobalt-nickel-iron-copper high entropy alloy nanoparticles. The present invention uses cake-shaped graphene oxide to soak the precursor salt solution and then dry it, which ensures the uniformity of distribution of each element in the precursor salt on the surface of the cake-shaped graphene oxide, prevents element segregation, and controls the phase composition of the platinum-cobalt-nickel-iron-copper high entropy alloy nanoparticles. Therefore, the graphene-supported platinum-cobalt-nickel-iron-copper high entropy alloy nanoparticles have the advantages of high specific surface area, many active sites and good stability, and have application potential in the fields of catalytic materials, superconducting materials, sensor materials and biomaterials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nano multi-element alloy preparation, and specifically relates to a method for preparing graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles. Background Art

[0002] Platinum-based high-entropy alloy nanoparticles have excellent physical and chemical properties, and are expected to become new multi-component catalysts with high activity, high selectivity, high stability and long service life due to the diversity of components, complexity of surface atomic structure, high mixing entropy and nanoscale effects. They have attracted much attention from researchers and are believed to have great application potential in the fields of electronics, catalysis and biology. Currently, nanoscale multi-component alloys are mainly prepared by liquid phase chemical methods due to the limitations of preparation methods. It is difficult to prepare nanoscale multi-component alloys with more than four elements, so there are still huge challenges in the preparation of high-entropy alloy nanoparticles.

[0003] High entropy alloy was first proposed by Professor Ye Junwei, a scholar from Taiwan. Later generations combined high entropy alloy with nanoparticles and found that it has very excellent physical and chemical properties. This is because it has the characteristics of high entropy alloy (high entropy effect, atomic hysteresis diffusion effect, severe lattice distortion effect, cocktail effect and high temperature stability effect) and nanoparticle characteristics (surface and interface effect, small size effect, quantum size effect and macroscopic quantum tunneling effect).

[0004] At present, the main preparation methods of multi-component alloys are: vacuum melting, powder metallurgy, mechanical alloying, laser cladding and electrochemical deposition. The prepared multi-component alloys are mainly in block or film form. The above methods are not suitable for the preparation of high-entropy alloy nanoparticles. Therefore, the preparation of high-entropy alloy nanoparticles has always been a difficulty in research in this field.

[0005] The patent with the publication number CN111545767A discloses a method for preparing a nanoscale multi-element alloy, which prepares a series of high entropy alloy nanoparticles, including the following steps: 1. Adding a precursor to ultrapure water to prepare a precursor steady-state solution; 2. Spray drying the precursor steady-state solution to obtain a precursor powder; 3. Calcining the precursor powder to obtain a nanoscale multi-element alloy. The method spray-dries and calcines the precursor steady-state solution to make the metals in the nanoparticles evenly distributed, forming a single-phase solid solution structure or a two-phase structure, and obtains nanoscale multi-element alloys or high entropy alloy nanoparticles composed of nanoparticles with a porous structure composed of any combination of fourteen metals. Although the method can systematically prepare high entropy alloy nanoparticles, the high entropy alloy nanoparticles have several structures, and the physical phase of the product is not easy to control.

[0006] The patent with publication number CN109295373A discloses an application of a multi-element alloy as a binder phase of tungsten carbide hard alloy and a preparation method of the tungsten carbide hard alloy, wherein CoCrCuFeNiMo is prepared by mixing Co powder, Cr powder, Cu powder, Fe powder, Ni powder and Mo powder, and then ball milling, drying and sieving. x Multicomponent alloy powder; then the prepared high entropy alloy powder, ball milling aid and WC powder are mixed, and high hardness tungsten carbide cemented carbide is obtained after ball milling, pressing and sintering. The multicomponent alloy prepared by this method is a powder and does not have a nanostructure, so it is not suitable for preparing nanoscale multicomponent alloys.

[0007] The patent with the publication number of CN112077331A discloses a method for preparing a carbon material-supported nanoscale multi-element alloy. The patent systematically describes the preparation process of carbon-supported high entropy alloy nanoparticles, including the following steps: 1. Add the selected carbon carrier and the prepared precursor salt to deionized water to prepare a steady-state colloidal solution; 2. Atomize and dry the steady-state colloidal precursor solution to obtain a carbon material-supported precursor nanoparticle powder; 3. Atomize and reduce the carbon material-supported precursor nanoparticle powder to finally obtain a carbon material-supported nanoscale multi-element alloy and high entropy alloy powder. The method mixes the carbon material carrier and the precursor salt and atomizes and dries them, so that the precursor salt forms nanoparticles and is uniformly loaded on the surface of the carbon material, and each element is uniformly distributed in the nanoparticles. Finally, the carbon material-supported precursor nanoparticle powder is calcined and reduced to obtain nanoscale multi-element alloys and high entropy alloys. The multi-element alloy and high entropy alloy nanoparticles are uniformly dispersed on the surface of the carbon material carrier and form a single-phase or multi-phase structure. However, the preparation process is complicated, the single preparation amount is limited, the atomization and drying process is difficult to control, and the particle size of the prepared material is uncontrollable. Summary of the invention

[0008] The technical problem to be solved by the present invention is to provide a method for preparing graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles in view of the deficiencies of the above-mentioned prior art. The method adopts a cake-shaped graphene oxide soaked in a precursor salt solution and then dried, thereby ensuring the uniformity of distribution of each element in the precursor salt on the surface of the cake-shaped graphene oxide, preventing element segregation, and then controlling the phase composition of the platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles in the product. Therefore, the graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles have the advantages of high specific surface area, multiple active sites and good stability, and solves the size and phase composition control problems of existing high-entropy alloy nanoparticles.

[0009] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles, characterized in that the method comprises the following steps:

[0010] Step 1: Prepare a solution of precursor salts of five elements, namely, platinum, cobalt, nickel, iron and copper, and stir them ultrasonically until they are completely dissolved to obtain a platinum-cobalt-nickel-iron-copper precursor salt solution, and then immerse the freeze-dried cake-shaped graphene oxide in the platinum-cobalt-nickel-iron-copper precursor salt solution;

[0011] Step 2: Take out and dry the cake-shaped graphene oxide soaked in step 1 to obtain graphene oxide wrapped in precursor salt, and then perform hydrogen calcination reduction to obtain graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles.

[0012] The invention prepares a precursor salt of a metal element in a target product into a platinum-cobalt-nickel-iron-copper precursor salt solution, then adds the solution into a cake-shaped graphene oxide for soaking, and adopts a cake-shaped graphene oxide with a certain shape as a matrix, which is not only convenient to operate, but also utilizes the hydrophilic oxygen-containing functional groups on the surface of the cake-shaped graphene oxide to adsorb the platinum-cobalt-nickel-iron-copper precursor salt solution on the surface of the cake-shaped graphene oxide, and after being taken out and dried, the platinum-cobalt-nickel-iron-copper precursor salt uniformly coats the cake-shaped graphene oxide, and forms a platinum-cobalt-nickel-iron-copper precursor salt with uniform composition on the surface of the cake-shaped graphene oxide, thereby preventing element segregation in a subsequent calcination reduction process, and effectively controlling the physical phase composition of platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles in the product graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles.

[0013] The above-mentioned method for preparing graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles is characterized in that the total metal ion concentration of the precursor salt in the platinum-cobalt-nickel-iron-copper precursor salt solution in step 1 is 0.01 mol / L, and the mass of the freeze-dried cake-shaped graphene oxide is 2.5 times the total mass equivalent of the metal elements in the platinum-cobalt-nickel-iron-copper precursor salt solution. The above-mentioned total metal ion concentration ensures that the elements in the platinum-cobalt-nickel-iron-copper precursor salt solution are evenly distributed, and the addition of the cake-shaped graphene oxide ensures that the precursor salt is evenly adsorbed, forming a cake-shaped graphene oxide uniformly coated with a uniformly mixed platinum-cobalt-nickel-iron-copper precursor salt.

[0014] The above-mentioned method for preparing graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles is characterized in that the immersion temperature in step one is 5°C to 35°C, and the immersion time is 4h to 24h.

[0015] The above-mentioned method for preparing graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles is characterized in that the drying temperature in step 2 is 40° C. to 70° C., and the immersion time is 1 h to 2 h.

[0016] The above-mentioned method for preparing graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles is characterized in that the temperature of the hydrogen calcination reduction in step 2 is 300°C to 600°C, and the time is 2h to 4h. By controlling the temperature and time of the hydrogen calcination reduction, it is ensured that the platinum-cobalt-nickel-iron-copper precursor salt uniformly coats the cake-shaped graphene oxide and is completely reduced to the graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles, while preventing the high-entropy alloy nanoparticles from agglomerating and having a phase separation structure.

[0017] The above-mentioned method for preparing graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles is characterized in that the mass content of each metal element in the graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles described in step 2 is greater than 5%, and is evenly distributed on the graphene surface, the average particle size of the platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles is 1nm to 10nm, and the phase structure is a face-centered cubic structure. The phase structure of the graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles in the present invention is a face-centered cubic structure, which ensures the structural stability of the platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles, thereby ensuring the stability of their performance, and at the same time having a large specific surface area, further improving the application performance of the graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles.

[0018] Compared with the prior art, the present invention has the following advantages:

[0019] 1. The present invention soaks cake-shaped graphene oxide in a precursor salt solution and then dries it, thereby ensuring the uniformity of distribution of elements in the precursor salt on the surface of the cake-shaped graphene oxide, preventing element segregation, and further controlling the phase composition of platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles in the product. Therefore, graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles have the advantages of high specific surface area, many active sites and good stability, and have excellent application potential in the fields of catalytic materials, superconducting materials, sensor materials and biomaterials.

[0020] 2. The mass content of each metal element in the graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles prepared by the present invention is greater than 5%, the average particle size of the platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles is 1nm to 10nm, they are evenly distributed on the graphene surface, and the physical structure is a face-centered cubic structure, and the structural and performance stability are improved.

[0021] 3. The preparation method of the present invention is simple, easy to implement, green and environmentally friendly, and suitable for industrial production.

[0022] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The present invention is a flow chart of the preparation process of graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles.

[0024] Figure 2 This is a TEM image of graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles prepared in Example 1 of the present invention.

[0025] Figure 3 This is the XRD pattern of graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0026] Example 1

[0027] like Figure 1 As shown, this embodiment includes the following steps:

[0028] Step 1, according to the atomic ratio of platinum, cobalt, nickel, iron, and copper of 1:1:1:1:1, ammonium chloroplatinate, cobalt chloride, nickel chloride, ferric chloride, and copper chloride are weighed to prepare a solution with a total metal ion concentration of 0.01 mol / L, and ultrasonically stirred until completely dissolved to obtain a platinum-cobalt-nickel-iron-copper precursor salt solution, and then freeze-dried cake-shaped graphene oxide is added according to twice the total mass equivalent of the metal elements in the platinum-cobalt-nickel-iron-copper precursor salt solution, and immersed at 5°C for 4h;

[0029] Step 2: Take out the soaked cake-shaped graphene oxide in step 1 and dry it at 40°C for 1 hour to obtain graphene oxide wrapped in precursor salt, then place it in a tubular furnace, and calcine and reduce it at 300°C in a hydrogen atmosphere for 2 hours to obtain graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles.

[0030] After testing, the atomic ratio of each metal element in the graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles prepared in this embodiment is 1:1:1:1:1, the average particle size of the platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles is 4 nm, and they are evenly distributed on the graphene surface, and the physical phase structure is a face-centered cubic structure.

[0031] Figure 2 TEM image of graphene-supported platinum-cobalt-nickel-iron-copper high entropy alloy nanoparticles prepared in this embodiment. Figure 2 It can be seen that the particle size of the platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles is less than 10 nm and is evenly distributed on the graphene surface.

[0032] Figure 3 The XRD pattern of the graphene-supported platinum-cobalt-nickel-iron-copper high entropy alloy nanoparticles prepared in this embodiment is shown in FIG. Figure 3 It can be seen that the platinum-cobalt-nickel-iron-copper high entropy alloy nanoparticles have a single-phase face-centered cubic structure.

[0033] Example 2

[0034] like Figure 1 As shown, this embodiment includes the following steps:

[0035] Step 1, according to the atomic ratio of platinum, cobalt, nickel, iron and copper of 1:1:1:1:1, ammonium chloroplatinate, cobalt chloride, nickel chloride, ferric chloride and cupric chloride are weighed to prepare a solution with a total metal ion concentration of 0.01 mol / L, and ultrasonically stirred until completely dissolved to obtain a platinum cobalt nickel iron copper precursor salt solution, and then freeze-dried cake-shaped graphene oxide is added according to 2.5 times the total mass equivalent of the metal elements in the platinum cobalt nickel iron copper precursor salt solution, and immersed at 35°C for 24 hours;

[0036] Step 2: Take out the soaked cake-shaped graphene oxide in step 1 and dry it at 70°C for 2 hours to obtain graphene oxide wrapped in precursor salt, then place it in a tubular furnace, and calcine and reduce it at 600°C in a hydrogen atmosphere for 4 hours to obtain graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles.

[0037] After testing, the atomic ratio of each metal element in the graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles prepared in this embodiment is 1:1:1:1:1, the average particle size of the platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles is 6 nm, and they are evenly distributed on the graphene surface, and the physical phase structure is a face-centered cubic structure.

[0038] Example 3

[0039] like Figure 1 As shown, this embodiment includes the following steps:

[0040] Step 1, according to the atomic ratio of platinum, cobalt, nickel, iron and copper of 1:1:1:1:1, ammonium chloroplatinate, cobalt chloride, nickel chloride, ferric chloride and cupric chloride are weighed to prepare a solution with a total metal ion concentration of 0.01 mol / L, and ultrasonically stirred until completely dissolved to obtain a platinum cobalt nickel iron copper precursor salt solution, and then freeze-dried cake-shaped graphene oxide is added according to twice the total mass equivalent of the metal elements in the platinum cobalt nickel iron copper precursor salt solution, and soaked at 25°C for 10 hours;

[0041] Step 2: Take out the soaked cake-shaped graphene oxide in step 1 and dry it at 50°C for 1.5 hours to obtain graphene oxide wrapped in precursor salt, then place it in a tubular furnace, and calcine and reduce it at 500°C in a hydrogen atmosphere for 3 hours to obtain graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles.

[0042] After testing, the atomic ratio of each metal element in the graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles prepared in this embodiment is 1:1:1:1:1, the average particle size of the platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles is 4.5 nm, and they are evenly distributed on the graphene surface, and the physical phase structure is a face-centered cubic structure.

[0043] Example 4

[0044] like Figure 1 As shown, this embodiment includes the following steps:

[0045] Step 1, according to the atomic ratio of platinum, cobalt, nickel, iron, and copper of 1:1:1:1:1, ammonium chloroplatinate, cobalt chloride, nickel chloride, ferric chloride, and copper chloride are weighed to prepare a solution with a total metal ion concentration of 0.01 mol / L, and ultrasonically stirred until completely dissolved to obtain a platinum-cobalt-nickel-iron-copper precursor salt solution, and then freeze-dried cake-shaped graphene oxide is added according to 2.5 times the total mass equivalent of the metal elements in the platinum-cobalt-nickel-iron-copper precursor salt solution, and soaked at 35° C. for 12 hours;

[0046] Step 2: Take out the soaked cake-shaped graphene oxide in step 1 and dry it at 70°C for 2 hours to obtain graphene oxide wrapped in precursor salt, then place it in a tubular furnace and calcine and reduce it at 500°C in a hydrogen atmosphere for 4 hours to obtain graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles.

[0047] After testing, the atomic ratio of each metal element in the graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles prepared in this embodiment is 1:1:1:1:1, the average particle size of the platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles is 10 nm, and they are evenly distributed on the graphene surface, and the physical phase structure is a face-centered cubic structure.

[0048] Example 5

[0049] like Figure 1 As shown, this embodiment includes the following steps:

[0050] Step 1, according to the atomic ratio of platinum, cobalt, nickel, iron, and copper of 1:1:1:1:1, ammonium chloroplatinate, cobalt chloride, nickel chloride, ferric chloride, and cupric chloride are weighed to prepare a solution with a total metal ion concentration of 0.01 mol / L, and ultrasonically stirred until completely dissolved to obtain a platinum-cobalt-nickel-iron-copper precursor salt solution, and then freeze-dried cake-shaped graphene oxide is added according to 2.5 times the total mass equivalent of the metal elements in the platinum-cobalt-nickel-iron-copper precursor salt solution, and immersed at 15°C for 4 hours;

[0051] Step 2: Take out the soaked cake-shaped graphene oxide in step 1 and dry it at 60°C for 2 hours to obtain graphene oxide wrapped in precursor salt, then place it in a tubular furnace and calcine and reduce it at 300°C in a hydrogen atmosphere for 2 hours to obtain graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles.

[0052] After testing, the atomic ratio of each metal element in the graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles prepared in this embodiment is 1:1:1:1:1, the average particle size of the platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles is 1 nm, and they are evenly distributed on the graphene surface, and the physical phase structure is a face-centered cubic structure.

[0053] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing graphene-supported platinum-cobalt-nickel-iron-copper high entropy alloy nanoparticles, characterized in that: The method comprises the following steps: Step 1: Prepare a solution of precursor salts of five elements, namely, platinum, cobalt, nickel, iron and copper, and stir them ultrasonically until they are completely dissolved to obtain a platinum-cobalt-nickel-iron-copper precursor salt solution, and then immerse the freeze-dried cake-shaped graphene oxide in the platinum-cobalt-nickel-iron-copper precursor salt solution; Step 2: Take out and dry the cake-shaped graphene oxide after soaking in step 1 to obtain graphene oxide wrapped by precursor salt, and then perform hydrogen calcination reduction to obtain graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles; the mass content of each metal element in the graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles is greater than 5%, and is evenly distributed on the surface of the graphene, the average particle size of the platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticles is 1nm-10nm, and the physical phase structure is a face-centered cubic structure.

2. The method for preparing graphene-supported platinum-cobalt-nickel-iron-copper high entropy alloy nanoparticles according to claim 1, characterized in that: The total metal ion concentration of the precursor salt in the platinum-cobalt-nickel-iron-copper precursor salt solution in step 1 is 0.01 mol / L, and the mass of the freeze-dried cake-shaped graphene oxide is 2.5 times the total mass equivalent of the metal elements in the platinum-cobalt-nickel-iron-copper precursor salt solution.

3. The method for preparing a graphene-supported platinum-cobalt-nickel-iron-copper high-entropy alloy nanoparticle according to claim 1, characterized in that: The soaking temperature in step 1 is 5° C. to 35° C., and the soaking time is 4 h to 24 h.

4. The method for preparing a graphene-supported platinum-cobalt-nickel-iron-copper high entropy alloy nanoparticle according to claim 1, characterized in that: The drying temperature in step 2 is 40° C. to 70° C., and the soaking time is 1 h to 2 h.

5. The method for preparing a graphene-supported platinum-cobalt-nickel-iron-copper high entropy alloy nanoparticle according to claim 1, characterized in that: The temperature of the hydrogen calcination reduction in step 2 is 300° C. to 600° C., and the time is 2 h to 4 h.