Synthesis method and application of amine imine nickel complex

By designing asymmetric nickel catalysts, the problem of insufficient copolymerization of ethylene and polar monomers in the prior art was solved, and efficient catalytic ethylene polymerization and copolymerization was achieved, and high performance with narrow molecular weight distribution and excellent mechanical properties were obtained. Polyolefin material.

CN115806572BInactive Publication Date: 2024-11-26ZHENGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211467061.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-22
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing catalysts are rarely used in catalytic copolymerization of ethylene and polar monomers, and it is difficult to obtain high-performance polyolefin materials with narrow molecular weight distribution and excellent mechanical properties.

Method used

An asymmetric amine imine nickel catalyst is designed to form an amine imine nickel complex by reacting with (DME)NiBr2 in an organic solvent to catalyze the homopolymerization of ethylene and polar monomers, with preferred conditions From -78°C to 200°C, the polymerization pressure is 0.01 to 10.0MPa.

Benefits of technology

High-efficiency catalytic ethylene polymerization and copolymerization is achieved, and high-performance polyolefin materials with narrow molecular weight distribution, high molecular weight and excellent mechanical properties are obtained. They have high catalytic activity and are suitable for various polar monomers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115806572B_ABST
    Figure CN115806572B_ABST
Patent Text Reader

Abstract

The present invention relates to a synthesis method and application of an aminoimine nickel complex. The structural formula of the complex is shown in formula (I): #imgabs0# The nickel complex provided by the present invention is used as a catalyst to catalyze ethylene homopolymerization or ethylene and polar olefin copolymerization to produce polyolefins with adjustable molecular weight and degree of branching. The aminoimine nickel catalyst provided by the present invention, under the action of a co-catalyst, efficiently catalyzes ethylene polymerization to obtain a high-performance polyolefin material with a narrow molecular weight distribution, a high molecular weight, and excellent mechanical properties. At the same time, under the action of side-arm heteroatoms, this type of catalyst effectively catalyzes the copolymerization of ethylene and various polar monomers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalysts, and in particular to a synthesis method and application of an aminoimine nickel complex. Background Art

[0002] Polyolefin is one of the indispensable materials in contemporary life. The development of new catalysts is the key to synthesizing high-performance polyolefin materials, and the design of ligands is crucial in the development of catalysts. Transition metal catalysts synthesized based on various ligands have played a key role in the field of olefin polymerization. Among the many ligands, Brookhart-type diimines are one of the most common structures. Compared with diimines post-transition metal catalysts, aminoimines catalyze olefin polymerization to obtain polyolefins with narrower molecular weight distribution (Chem. Commun., 2012, 48, 3312–3314). However, there are few examples of this type of catalyst in catalyzing the copolymerization of ethylene and polar monomers (Polym. Chem., 2016, 7, 529–537).

[0003] The present invention designs and synthesizes a series of asymmetric amine-imine nickel catalysts, which can efficiently catalyze ethylene polymerization under the action of a co-catalyst to obtain high-performance polyolefin materials: narrow molecular weight distribution, high molecular weight, and excellent mechanical properties. At the same time, this type of catalyst can effectively catalyze the copolymerization of ethylene and various polar monomers under the action of side-arm heteroatoms. Summary of the invention

[0004] In view of the problems existing in the prior art, the present invention provides a synthesis method and application of an aminoimine nickel complex. The aminoimine nickel complex is used as a catalyst for ethylene homopolymerization or ethylene and polar monomer copolymerization, has high catalytic activity, and obtains a high-performance polyolefin material.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0006] The present invention provides an asymmetric amine-imine nickel metal catalyst having a structure of formula (I):

[0007]

[0008] R1 is CH3, i Pr or CHPh2;

[0009] R2 is CH3, i Pr or CHPh2;

[0010] R3 is CH3 or H;

[0011] —: refers to covalent bond or coordination bond;

[0012] ---: refers to bonding or non-bonding.

[0013] The synthesis method of nickel metal catalyst comprises the following steps: in an organic solvent, the following ligand formula (II) is mixed with (DME)NiBr2 and reacted for a period of time to obtain the catalyst.

[0014]

[0015] Wherein: R1, R2, R3 are the same as those described in Formula I.

[0016] The structural formula of some of the aminoimine compounds used in the catalyst of the present invention is as follows:

[0017]

[0018] The structural formula of the amidoimine nickel complex of some catalysts of the present invention is as follows:

[0019]

[0020] In the above process of preparing the nickel complex, the organic solvent is an organic solvent well known to those skilled in the art, preferably the organic solvent is a halogenated alkane, more preferably the organic solvent is one or more of chloroform, dichloromethane and 1,2-dichloroethane. The molar ratio of the ligand to the nickel compound is 1:(0.1-6), and in a specific embodiment, the molar ratio of the ligand to the nickel compound is 1:(1-3). The temperature is carried out at -78°C to 200°C. The reaction time is 1-50h; in a specific embodiment, the reaction time is 12-24h.

[0021] The preparation method of the aminoimine compound represented by formula II of the present invention is as follows: the structure represented by formula III undergoes a condensation reaction with an amine compound under the catalysis of an acid to generate the aminoimine compound represented by formula II. The reaction route is as follows:

[0022]

[0023] R1, R2, and R3 in Formula IV have the same definitions as in Formula I.

[0024] The preparation method of the compound of the structure shown in Formula III of the present invention is that under the catalysis of a base, the α-bromoketone shown in Formula V reacts with the o-methoxyaniline shown in Formula VI to obtain the aminoketone compound shown in Formula III. The reaction route is as follows:

[0025]

[0026] An ethylene polymerization method, under the catalytic action of the aminoimine nickel complex of the present invention, carries out ethylene polymerization reaction, preferably, the polymerization reaction temperature is -78 DEG C to 200 DEG C, and the polymerization pressure is 0.01 to 10.0 MPa.

[0027] A preparation method for copolymerization of ethylene and polar monomers, wherein ethylene and polar monomers are copolymerized under the catalytic action of the aminoimine nickel complex of the present invention to obtain a copolymer. Preferably, the polymerization reaction temperature is -78°C to 200°C, and the polymerization pressure is 0.01 to 10.0 MPa.

[0028] The polar monomer in the present invention refers to an α-olefin containing a heteroatom, including 10-enoic acid methyl ester, 10-undecenoic acid, 10-undecenol, 6-chlorohexene, methyl acrylate, ethyl acrylate, propylene acetate, methyl norbornene, and the like.

[0029] The above-mentioned olefin copolymerization or homopolymerization process is well known to those skilled in the art and will not be described in detail here; the difference is that the catalyst used in the above-mentioned olefin polymerization is the nickel complex provided by the present invention. The experimental results show that the nickel complex provided by the present application has high catalytic activity for olefin polymerization and can produce high-performance polyolefin materials with adjustable molecular weight distribution and branching degree.

[0030] Beneficial effects of the invention: The invention relates to a method for synthesizing an asymmetric amine-imine nickel catalyst. The catalyst can efficiently catalyze ethylene polymerization to obtain a high-performance polyolefin material with a narrow molecular weight distribution, a high molecular weight, and excellent mechanical properties. At the same time, the catalyst can effectively catalyze the copolymerization of ethylene and various polar monomers under the action of side-arm heteroatoms. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is the single crystal structure of the nickel-imide compound I1.

[0032] Figure 2 This is the single crystal structure of the nickel-imide compound I2.

[0033] Figure 3 This is the single crystal structure of the nickel-imide compound I3.

[0034] Figure 4 This is the single crystal structure of the nickel-imide compound I4. DETAILED DESCRIPTION

[0035] The present invention is further described below in conjunction with specific examples. It should be understood that the following examples are helpful for further understanding of the present invention, but do not limit the scope of the present invention, and those skilled in the art can make some non-essential improvements and adjustments based on the content of the above invention.

[0036] The following examples show different aspects of the present invention. The data provided include the synthesis of ligands, the synthesis of metal complexes, polymerization operations, polymerization conditions and polymer products. All operations including reactions, preparations and storages were carried out under a dry inert atmosphere using standard Schlenk operations. Molecular weight and molecular weight distribution were determined using the Malvern GPC instrument. The instrument was equipped with a dual detection array including a differential refractive index (RI) detector and a two-angle light scattering (LS) detector. The LS detector detection angles were 15 and 90, respectively, the laser wavelength was 658 nm, THF was used as the eluent, and the flow rate was 1.0 mL / min.

[0037] Example 1

[0038] The synthesis method of the structural compound described in Formula III of this embodiment is as follows:

[0039] In a 50mL Shrek bottle, add 3-bromo-3-methyl-2-butanone (V) (1.34mL, 11mmol), o-anisidine (1.13mL, 10mmol), magnesium oxide (0.20mg, 5.0mmol), 10mL N,N-dimethylformamide (DMF), react at 50℃ for 24h, cool to room temperature, extract with ethyl acetate and concentrate to obtain a crude product, separate by column chromatography (petroleum ether / ethyl acetate = 50 / 1) to obtain a light yellow solid III, 1.38g (67%). Experimental data of this compound: 1 H NMR (600MHz, CDCl3): δ6.79 (dd, J=7.9, 1.3Hz, 1H), 6.76 (td, J=7.7, 1.4Hz, 1H), 6.67 (td, J=7.7, 1.5Hz, 1H), 6.25(dd,J=7.8,1.4Hz,1H),4.58(s,1H,NH),3.86(s,3H,OCH3),2.21(s,3H,N=CCH3),1.44(s,6H,C(CH3)2). 13 C NMR (151MHz, CDCl3): δ214.6,146.9,135.1,121.0,117.1,111.1,109.7,61.6,55.4,24.6,24.1.HRMS(ESI-TOF)m / z:[M+H] + Calculate for C 12 H 18 N2O + ,208.1332,found,208.1334.

[0040] Example 2

[0041] The synthesis method of the aminoimine compound II1 in this embodiment is as follows:

[0042] In a 100 mL round-bottom flask, compound III (1.05 g, 4 mmol), 2,6-diisopropylaniline (1.06 g, 6.0 mmol), p-toluenesulfonic acid (0.69 g, 4 mmol), and 60 mL of toluene were added, heated, and refluxed in a water separator for 24 h, then cooled to room temperature, filtered, and concentrated to obtain a crude product, which was separated by column chromatography (petroleum ether / ethyl acetate = 100 / 1) to obtain a white solid aminoimine compound II1, 1.29 g (44%). Experimental data of this compound: 1 H NMR (600MHz, CDCl3): δ7.13(d,J=7.6Hz,2H),7.5(t,J=7.6Hz,1H),6.84-6.81( m,2H),6.74(dd,J=7.8,1.5Hz,1H),6.69(td,J=7.8,1.5Hz,1H),4.80(1H,NH),3 .88(s,3H,OCH3),2.82(septet,2H,CH(CH3)2),1.72(s,3H,N=CCH3),1.69(s,6 H,C(CH3)2),1.23(d,J=6.8Hz,6H,CH(CH3)2),1.17(d,J=6.8Hz,6H,CH(CH3)2). 13 C NMR (151MHz, CDCl3): δ176.7,146.9,146.3,136.0,135.9,123.1,122.8,120.7,116.5,111.6,1 09.7,59.4,55.5,55.4,29.7,28.0,26.79,26.77,23.1,15.71,15.70.HRMS(ESI-TOF)m / z:[M+H] + Calculate for C 24 H 35 N2O + ,367.2744,found,366.2742.

[0043] Example 3

[0044] The synthesis method of the aminoimine compound II2 of this embodiment is as follows:

[0045] In a 100 mL round-bottom flask, compound III (1.05 g, 4 mmol), 2,6-dimethylaniline (0.73 g, 6.0 mmol), p-toluenesulfonic acid (0.69 g, 4 mmol), and 60 mL of toluene were added, heated, and refluxed in a water separator for 24 h, then cooled to room temperature, filtered, and concentrated to obtain a crude product, which was separated by column chromatography (petroleum ether / ethyl acetate = 100 / 1) to obtain a white solid aminoimine compound II2, 0.66 g (53%). Experimental data of this compound: 1 H NMR (600MHz, CDCl3): δ7.01 (d, J = 7.4Hz, 2H), 6.87 (t, J = 7.4Hz, 1H), 6.81-6.72 (m, 3H), 6. 66(t,J=7.3Hz,1H),4.69(s,1H,NH),3.87(s,3H,OCH3),2.07(s,6H,ArCH3),1.67(s,9H). 13 C NMR (151MHz, CDCl3): δ177.5,148.7,146.8,135.8,128.1,125.6,122.6,120.8 ,116.5,111.8,109.6,59.3,55.4,26.9,18.3,15.1.HRMS(ESI-TOF)m / z:[M+H] + Calculate for C 20 H 27 N2O + ,311.2118,found,311.2116.

[0046] Example 4

[0047] The synthesis method of the aminoimine compound II3 of this embodiment is as follows:

[0048] In a 100 mL round-bottom flask, compound III (1.05 g, 4 mmol), 2-dibenzhydryl-4,6-dimethylaniline (1.72 g, 6.0 mmol), p-toluenesulfonic acid (0.69 g, 4 mmol), and 60 mL of toluene were added respectively, heated, refluxed in a water separator for 24 h, cooled to room temperature, filtered and concentrated to obtain a crude product, and separated by column chromatography (petroleum ether / ethyl acetate = 100 / 1) to obtain a white solid aminoimine compound II2, 0.72 g (38%). Experimental data of this compound: 1H NMR (600MHz, CDCl3): δ7.25-7.20 (m, 4H), 7.16 (dt, J = 13.1, 7.2Hz, 2H), 7.05 (dd, J=17.3,7.3Hz,4H),6.87(s,1H),6.77-6.69(m,3H),6.62(td,J=7.7,1.7Hz,1H), 6.57(s,1H),5.52(s,1H,CHPh2),4.96(s,1H,NH),3.82(s,3H,OCH3),2.18(s,3H, ArCH3),2.02(s,3H,ArCH3),1.56(s,3H,N=CCH3),1.39(d,J=5.2Hz,6H,C(CH3)2). 13 C NMR (151MHz, CDCl3): δ177.85,147.07,145.55,144.61,143.48,135.84,13 2.06,131.55,129.82,129.55,129.51,128.65,128.10,128.07,126.09,125 .95,125.49,120.73,116.28,112.12,109.61,77.23,77.02,76.80,59.21, 55.45,51.21,27.79,25.34,20.95,18.70,15.42.HRMS(ESI-TOF)m / z:[M+H] + Calculate for C 23 H 37 N2O + ,477.2901,found,477.2905.

[0049] Example 5

[0050] The synthesis method of the aminoimine compound II4 in this embodiment is as follows:

[0051] In a 100 mL round-bottom flask, compound III (1.05 g, 4 mmol), 2,6-diphenylmethyl-4-methylaniline (2.64 g, 6.0 mmol), p-toluenesulfonic acid (0.69 g, 4 mmol), and 60 mL of toluene were added respectively, heated, refluxed in a water separator for 24 h, cooled to room temperature, filtered and concentrated to obtain a crude product, and separated by column chromatography (petroleum ether / ethyl acetate = 100 / 1) to obtain a white solid aminoimine compound II2, 0.53 g (21%). Experimental data of this compound: 1H NMR (600MHz, CDCl3): δ7.23(dd,J=12.8,7.4Hz,8H),7.18-7.15(m,4H),7.05(dd,J=17.0,7.4Hz,8H),6.76(d,J=7.8Hz,1H),6.74-6.64(m,4H) ,6.64-6.57(m,1H),5.43(s,2H,CHPh2),5.25(s,1H,NH),3.79(s,3H,OCH3),2.13(s,3H,ArCH3),1.35(s,6H,C(CH3)2),1.12(s,3H,,N=CCH3). 13 C NMR (151MHz, CDCl3): δ178.01,147.52,145.45,144.53,143.22,136.00,131.41,131.24,129.91,129.42,129.41,128.15,127.99,126. 14,125.91,120.80,116.32,112.43,109.85,77.22,77.01,76.80,59.30,55.53,51.09,26.42,21.25,16.10.HRMS(ESI-TOF)m / z:[M+H] + Calculate for C 45 H 45 N2O + ,629.3527,found,629.3531.

[0052] Example 6

[0053] The synthesis method of the amido-imine nickel compound I1 in this embodiment is as follows:

[0054] Under argon protection, add aminoimine compound II1 (0.37 g, 1.01 mmol), (DME)NiBr2 (0.31 g, 1.00 mmol), and 20 mL of anhydrous dichloromethane to a 50 mL reaction bottle, react at room temperature for 24 hours, filter, and concentrate. Recrystallize in dichloromethane and n-hexane solution, 0.47 g (80%). Experimental data of this compound: MALDI-TOF-MS (m / z): [M-Br] + Calculate for C 24 H 34 BrN2NiO + ,503.1203,found,503.1202. Elemental analysis: C 24 H 34Br2N2NiO: C, 49.27; H, 5.86; N, 4.79; Found: C, 49.02; H, 5.77; N, 4.35. The structure of the nickel-imide compound I1 was characterized by X-ray single crystal diffraction (see Appendix Figure 1 ).

[0055] Example 7

[0056] The synthesis method of the amido-imine nickel compound I2 of this embodiment is as follows:

[0057] Under argon protection, add aminoimine compound II2 (0.31 g, 1.01 mmol), (DME)NiBr2 (0.31 g, 1.00 mmol), and 20 mL of anhydrous dichloromethane to a 50 mL reaction bottle, react at room temperature for 36 hours, filter, and concentrate. Recrystallize in dichloromethane and n-hexane solution, 0.47 g (90%). Experimental data of this compound: MALDI-TOF-MS (m / z): [M-Br] + Calculate for C 20 H 26 BrN2NiO + ,447.0577,found,447.0570. Elemental analysis: C 20 H 26 Br2N2NiO: C, 45.42; H, 4.95; N, 5.30; Found: C, 45.02; H, 4.92; N, 5.15. The structure of the nickel-imide compound I2 was characterized by X-ray single crystal diffraction (see Appendix Figure 2 ).

[0058] Example 8

[0059] The synthesis method of the amido-imine nickel compound I3 of this embodiment is as follows:

[0060] Under argon protection, add aminoimine compound II3 (0.48 g, 1.01 mmol), (DME)NiBr2 (0.31 g, 1.00 mmol), and 20 mL of anhydrous dichloromethane to a 50 mL reaction bottle, react at room temperature for 36 hours, filter, and concentrate. Recrystallize in dichloromethane and n-hexane solution, 0.53 g (76%). Experimental data of this compound: MALDI-TOF-MS (m / z): [M-Br] + Calculate for C 33 H 36 BrN2NiO + ,613.1359,found,613.1362. Elemental analysis: C 33 H 36Br2N2NiO: C, 57.02; H, 5.22; N, 4.03; Found: C, 57.22; H, 5.15; N, 3.95. The structure of the nickel-imide compound I3 was characterized by X-ray single crystal diffraction (see Appendix Figure 3 ).

[0061] Example 9

[0062] The synthesis method of the amido-imine nickel compound I4 in this embodiment is as follows:

[0063] Under argon protection, add aminoimine compound II4 (0.64g, 1.01mmol), (DME)NiBr2 (0.31g, 1.00mmol), and 20mL of anhydrous dichloromethane to a 50mL reaction bottle, react at room temperature for 36h, filter and concentrate. Recrystallize in dichloromethane and n-hexane solution, 0.68g (72%). Experimental data of this compound: MALDI-TOF-MS (m / z): [M-Br] + Calculate for C 45 H 44 BrN2NiO + ,765.1985,found,765.1980.. Elemental analysis: C 45 H 44 Br2N2NiO: C, 63.79; H, 5.23; N, 3.31; Found: C, 63.10; H, 5.37; N, 3.01. The structure of the nickel-imide compound I4 was characterized by X-ray single crystal diffraction (see Appendix Figure 4 ).

[0064] Examples 10 to 19 show that the aminoimine nickel complex exhibits special catalytic characteristics in ethylene homopolymerization and ethylene and polar monomer copolymerization. Within a certain pressure range, it catalyzes ethylene polymerization with high activity to obtain high-performance polyolefin materials: narrow molecular weight distribution, high molecular weight, and excellent mechanical properties.

[0065] Example 10

[0066] Under anhydrous and oxygen-free conditions, dry toluene (45 mL) and Et2AlCl (3 mL, 1 M toluene solution) were added to a 350 mL thick-walled reaction bottle in sequence, ethylene was introduced until saturated, and then 2 mL (Al / Ti = 300) of dichloromethane solution of aminoimine nickel catalyst I1 (10 μmol) was added, 1 atm, and reacted at room temperature for 30 min. The reaction was terminated with ethanol containing 5% hydrochloric acid. After precipitation, filtration, and washing, the polymer was vacuum dried at 50 ° C to constant weight to obtain 1.60 g of polymerization product. The catalytic activity was 3.20×10 5 g PE mol -1h -1 The molecular weight of the obtained polymer is M n =1.12×10 5 g / mol, molecular weight distribution is 1.27, and degree of branching is 114.

[0067] Embodiment 11

[0068] Under anhydrous and oxygen-free conditions, dry toluene (48 mL) and Et2AlCl (0.3 mL, 1 M toluene solution) were added to a 350 mL thick-walled reaction bottle in sequence, ethylene was introduced until saturated, and then 2 mL (Al / Ti = 300) of dichloromethane solution of aminoimine nickel catalyst I1 (1 μmol) was added, and the reaction was carried out at 8 atm for 30 min at room temperature. The reaction was terminated with ethanol containing 5% hydrochloric acid. After precipitation, filtration, and washing, the polymer was vacuum dried at 50 ° C to constant weight to obtain 1.18 g of polymerization product. The catalytic activity was 2.36×10 6 g PE mol -1 h -1 The molecular weight of the obtained polymer is M n =4.14×10 5 g / mol, molecular weight distribution is 1.26, and degree of branching is 101.

[0069] Example 12

[0070] Under anhydrous and oxygen-free conditions, dry toluene (48 mL) and Et2AlCl (0.3 mL, 1 M toluene solution) were added to a 350 mL thick-walled reaction bottle in sequence, ethylene was introduced until saturated, and then 2 mL (Al / Ti = 300) of dichloromethane solution of aminoimine nickel catalyst I2 (1 μmol) was added, and the reaction was carried out at 8 atm for 30 min at room temperature. The reaction was terminated with ethanol containing 5% hydrochloric acid. After precipitation, filtration, and washing, the polymer was vacuum dried at 50 ° C to constant weight to obtain 0.73 g of polymerization product. The catalytic activity was 1.46×10 6 g PE mol -1 h -1 The molecular weight of the obtained polymer is M n =2.56×10 5 g / mol, molecular weight distribution is 1.28, and branching degree is 102. The mechanical properties of the polymer were studied, and the breaking strain value was 1610% and the breaking stress value was 4.83Mpa.

[0071] Example 13

[0072] Under anhydrous and oxygen-free conditions, dry toluene (48 mL) and Et2AlCl (0.3 mL, 1 M toluene solution) were added to a 350 mL thick-walled reaction bottle in sequence, ethylene was introduced until saturated, and then 2 mL (Al / Ti = 300) of dichloromethane solution of aminoimine nickel catalyst I3 (1 μmol) was added, 8 atm, and reacted at room temperature for 30 min. The reaction was terminated with ethanol containing 5% hydrochloric acid. After precipitation, filtration, and washing, the polymer was vacuum dried at 50 ° C to constant weight to obtain 1.47 g of polymerization product. The catalytic activity was 2.93×10 6 g PE mol -1 h -1 The molecular weight of the obtained polymer is M n =5.59×10 5 g / mol, molecular weight distribution is 1.27, and branching degree is 88. The mechanical properties of the polymer were studied, showing good elastomeric properties, with a breaking strain value of 830%, a breaking stress value of 13.3Mpa, and an elastic recovery rate of 75%.

[0073] Embodiment 14

[0074] Under anhydrous and oxygen-free conditions, dry toluene (48 mL) and Et2AlCl (0.3 mL, 1 M toluene solution) were added to a 350 mL thick-walled reaction bottle in sequence, and ethylene was introduced until saturated. Then, the mixture was placed in a 40°C metal bath and kept at a constant temperature for a certain period of time. Then, 2 mL of dichloromethane solution of aminoimine nickel catalyst I3 (1 μmol) (Al / Ti=300) was added, and the reaction was carried out at 8 atm for 30 min at room temperature. The reaction was terminated with ethanol containing 5% hydrochloric acid. After precipitation, filtration, and washing, the polymer was vacuum dried at 50°C to constant weight to obtain 1.74 g of a polymer product. The catalytic activity was 3.48×10 6 g PE mol -1 h -1 The molecular weight of the obtained polymer is M n =3.29×10 5 g / mol, molecular weight distribution is 1.36, and branching degree is 91. The mechanical properties of the polymer were studied, showing good elastomeric properties, with a breaking strain value of 1900%, a breaking stress value of 3.77Mpa, and an elastic recovery rate of 69%.

[0075] Embodiment 15

[0076] Under anhydrous and oxygen-free conditions, dry toluene (48 mL) and Et2AlCl (0.3 mL, 1 M toluene solution) were added to a 350 mL thick-walled reaction bottle in sequence, ethylene was introduced until saturated, and then 2 mL (Al / Ti = 300) of dichloromethane solution of aminoimine nickel catalyst I4 (5 μmol) was added, 8 atm, and reacted at room temperature for 30 min. The reaction was terminated with ethanol containing 5% hydrochloric acid. After precipitation, filtration, and washing, the polymer was vacuum dried at 50 ° C to constant weight to obtain 2.16 g of polymerization product. The catalytic activity was 8.63×10 5 g PE mol -1 h -1 The molecular weight of the obtained polymer is M n =2.15×10 5 g / mol, molecular weight distribution is 1.30, and branching degree is 83. The mechanical properties of the polymer were studied, showing good elastomeric properties, with a breaking strain value of 890% and a breaking stress value of 6.07Mpa.

[0077] Example 16

[0078] Under anhydrous and oxygen-free conditions, dry toluene and Et2AlCl (3 mL, 1 M toluene solution) were added to a 350 mL thick-walled reaction bottle in sequence, ethylene was introduced until saturated, and then 1 mL (Al / Ti=300) of dichloromethane solution of aminoimine nickel catalyst I3 (10 μmol) and 6-chlorohexene (1 M) were added. The reaction volume was maintained at 20 mL, 1 atm, and the reaction was carried out at room temperature for 1 h. The reaction was terminated with ethanol containing 5% hydrochloric acid. After precipitation, filtration, and washing, the polymer was vacuum dried at 50 ° C to constant weight to obtain 0.52 g of polymerization product. The catalytic activity was 5.2×10 4 g PE mol -1 h -1 The molecular weight of the obtained polymer is M n =3.37×10 4 g / mol, the molecular weight distribution is 2.00, the branching degree is 78, and the insertion rate is 1.64%.

[0079] Embodiment 17

[0080] Under anhydrous and oxygen-free conditions, dry toluene and Et2AlCl (6 mL, 1 M toluene solution) were added to a 350 mL thick-walled reaction bottle in sequence, ethylene was introduced until saturated, and then 1 mL (Al / Ti=300) of dichloromethane solution of aminoimine nickel catalyst I2 (20 μmol) and 10-enoic acid methyl ester (0.25 M) were added. The reaction volume was maintained at 20 mL, 1 atm, and the reaction was carried out at room temperature for 4 h. The reaction was terminated with ethanol containing 5% hydrochloric acid. After precipitation, filtration, and washing, the polymer was vacuum dried at 50 ° C to constant weight to obtain 1.79 g of polymerization product. The catalytic activity was 2.24×104 g PE mol -1 h -1 The molecular weight of the obtained polymer is M n =1.37×10 4 g / mol, the molecular weight distribution is 2.20, the branching degree is 108, and the insertion rate is 2.52%.

[0081] Embodiment 18

[0082] Under anhydrous and oxygen-free conditions, dry toluene and Et2AlCl (6 mL, 1 M toluene solution) were added to a 350 mL thick-walled reaction bottle in sequence, ethylene was introduced until saturated, and then 1 mL (Al / Ti=300) of dichloromethane solution of aminoimine nickel catalyst I3 (20 μmol) and 10-undecenoic acid (0.25 M) were added. The reaction volume was maintained at 20 mL, 1 atm, and the reaction was carried out at room temperature for 1 h. The reaction was terminated with ethanol containing 5% hydrochloric acid. After precipitation, filtration, and washing, the polymer was vacuum dried at 50 ° C to constant weight to obtain 2.52 g of the polymer product. The catalytic activity was 1.26×10 5 g PE mol -1 h -1 The molecular weight of the obtained polymer is M n =3.0×10 4 g / mol, the molecular weight distribution is 3.12, the branching degree is 80, and the insertion rate is 1.60%.

[0083] Embodiment 19

[0084] Under anhydrous and oxygen-free conditions, dry toluene and Et2AlCl (6 mL, 1 M toluene solution) were added to a 350 mL thick-walled reaction bottle in sequence, ethylene was introduced until saturated, and then 1 mL (Al / Ti=300) of dichloromethane solution of aminoimine nickel catalyst I3 (20 μmol) and 10-undecenol (0.25 M) were added. The reaction volume was maintained at 20 mL, 1 atm, and the reaction was carried out at room temperature for 1.5 h. The reaction was terminated with ethanol containing 5% hydrochloric acid. After precipitation, filtration, and washing, the polymer was vacuum dried at 50 ° C to constant weight to obtain 1.41 g of polymerization product. The catalytic activity was 4.7×10 4 g PE mol -1 h -1 The molecular weight of the obtained polymer is M n =9.33×10 4 g / mol, the molecular weight distribution is 2.37, the branching degree is 91, and the insertion rate is 1.08%.

[0085] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. An amine-imine nickel complex, the structural formula of which is shown in formula (I): R1 is CH3, i Pr or CHPh2; R2 is CH3, i Pr or CHPh2; R3 is CH3 or H.

2. The method for preparing the amidoimine nickel complex according to claim 1, characterized in that: An aminoimine compound is reacted with (DME)NiBr2 in an organic solvent to obtain an aminoimine nickel complex shown in formula (I); wherein DME is ethylene glycol dimethyl ether, and the structural formula of the aminoimine compound is shown in formula (II): ; In formula (II), R1 is CH3, i Pr or CHPh2; R2 is CH3, i Pr or CHPh2; R3 is CH3 or H.

3. The method for preparing the amidoimine nickel complex according to claim 2, characterized in that: The organic solvent is one or more of chloroform, dichloromethane and 1,2-dichloroethane; the molar ratio of the aminoimine compound to (DME)NiBr2 is 1:(0.1-6), the reaction temperature is -78°C to 200°C, and the reaction time is 1-50 h.

4. The method for preparing the amido-imine nickel complex according to claim 2, characterized in that: The preparation method of the aminoimine compound is: the aminoketone compound represented by formula (III) is subjected to a condensation reaction with the amine compound represented by formula (IV) under the catalysis of an acid to generate the aminoimine compound represented by formula (II). The reaction route is as follows: ; R1 in formula IV is CH3, i Pr or CHPh2; R2 is CH3, i Pr or CHPh2; R3 is CH3 or H.

5. The method for preparing the amidoimine nickel complex according to claim 4, characterized in that: The molar ratio of the amino ketone compound represented by formula (III) to the amine compound represented by formula (IV) is 2:3, and the water separator is heated to reflux for reaction for 24 hours.

6. The method for preparing the amidoimine nickel complex according to claim 4, characterized in that: The preparation method of the structural compound represented by formula (III) is as follows: under the catalysis of a base, the structural compound represented by formula (V) α -bromoketone reacts with o-anisidine represented by formula (VI) to obtain an aminoketone compound represented by formula (III); the reaction scheme is as follows: 。 7. The method for preparing the amidoimine nickel complex according to claim 6, characterized in that: The formula (V) α The molar ratio of the -bromoketone to the o-anisidine represented by formula (VI) is 2:1, the reaction temperature is 50°C, and the reaction time is 24 hours.

8. Use of the amido-imine nickel complex according to claim 1 as a catalyst in ethylene polymerization, characterized in that: The polymerization reaction temperature is -78°C to 200°C, and the polymerization reaction pressure is 0.01 to 10.0 MPa.

9. Use of the aminoimine nickel complex according to claim 1 as a catalyst in the copolymerization of ethylene and polar monomers, characterized in that: Under the catalytic action of the aminoimine nickel complex, ethylene and polar monomers are copolymerized to obtain a copolymer. The copolymerization reaction temperature is -78°C to 200°C, and the copolymerization reaction pressure is 0.01 to 10.0 MPa.

10. The use according to claim 9, characterized in that: The polar monomer is methyl norbornene or a heteroatom-containing α -olefins, the heteroatom-containing α - Olefin is 10-enoic acid methyl ester, 10-undecenoic acid, 10-undecenol, 6-chlorohexene, methyl acrylate, ethyl acrylate or propylene acetate.