Composite plastic woven fabric with infrared reflection function and preparation method and application thereof

The infrared reflective masterbatch composed of materials such as titanium dioxide and low-density polyethylene coated with nano-silicon dioxide, combined with white mineral oil, solves the problems of poor infrared reflection effect and poor waterproof performance in the prior art, and prepares excellent Composite plastic woven fabric with infrared reflection and waterproof properties is suitable for thermal insulation and waterproof applications in agricultural greenhouses and construction fields.

CN115807343BActive Publication Date: 2024-11-05FSPG HI TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211654832.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-22
Publication Date
2024-11-05
Estimated Expiration
2042-12-22

AI Technical Summary

Technical Problem

The existing film preparation process with infrared reflection function is complicated, the infrared reflection effect is poor, and the waterproof effect is poor.

Method used

The infrared reflective masterbatches consisting of nanosilicon dioxide coated with titanium dioxide and/or nanozirconium oxide, low-density polyethylene and linear low-density polyethylene are designed through extrusion granulation and braiding layer. A composite plastic woven fabric with infrared reflection function was prepared, and the upper and lower surfaces of the braided layer were coated with components of the upper and lower coating layer.

Benefits of technology

It significantly improves the infrared reflection function and waterproof performance of composite plastic woven fabrics, and is suitable for heat insulation and waterproof applications in agricultural greenhouses and construction fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115807343B_ABST
    Figure CN115807343B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of plastic technology, and particularly relates to a composite plastic woven cloth with infrared reflection function, a preparation method thereof and an application thereof. The composite plastic woven cloth comprises, from bottom to top, a lower coating layer, a woven layer and an upper coating layer in sequence; the upper coating layer comprises an infrared reflection masterbatch, and the infrared reflection masterbatch comprises, by weight, 10-30 parts of nano-silicon dioxide-coated titanium dioxide and / or nano-zirconium oxide, 60-80 parts of low-density polyethylene, and 4-12 parts of linear low-density polyethylene. The special components and content of the infrared reflection masterbatch enable the infrared reflection masterbatch to be added to the upper coating layer to interact with other components, thereby significantly improving the infrared reflection function and waterproof effect of the composite plastic woven cloth. For example, the reflectance ratio to near infrared exceeds 0.8.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of plastics, and in particular relates to a composite plastic woven cloth with infrared reflection function and a preparation method and application thereof. Background Art

[0002] Films with infrared reflection function are used in some electronic products or other fields. However, the preparation process of existing films with infrared reflection function is complicated and the infrared reflection effect is poor.

[0003] Prior art CN104024352A discloses infrared reflective film, infrared reflective coating and infrared reflector, the average infrared reflectivity at 780nm-2500nm is more than 7.5% (15μm-60μm transparent coating), and the average visible light transmittance at 380nm-780nm is more than 60%. That is, the existing infrared reflective film has poor infrared reflection effect.

[0004] In addition, the waterproof effect of the membrane material with infrared reflection function in the prior art is poor.

[0005] Therefore, there is an urgent need to provide a new plastic film material with infrared reflection function and further improve the waterproof effect of the plastic film material. Summary of the invention

[0006] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention proposes a composite plastic woven fabric with infrared reflection function and its preparation method and application. The composite plastic woven fabric of the present invention has good infrared reflection function and further has good waterproof effect. The composite plastic woven fabric of the present invention has good heat insulation effect in the field of agricultural greenhouses, and not only has heat insulation and cooling effect in the field of construction, but also has good waterproof effect.

[0007] A first aspect of the present invention provides a composite plastic woven fabric with infrared reflection function.

[0008] Specifically, a composite plastic woven fabric with infrared reflection function comprises, from bottom to top, a lower coating layer, a woven layer, and an upper coating layer;

[0009] The upper coating layer comprises infrared reflective masterbatch, which comprises, by weight, 10-30 parts of nano-silicon dioxide-coated titanium dioxide and / or nano-zirconium oxide, 60-80 parts of low-density polyethylene (LDPE), and 4-12 parts of linear low-density polyethylene (LLDPE).

[0010] Preferably, the infrared reflective masterbatch further comprises white mineral oil, which is not only beneficial to the preparation of the infrared reflective masterbatch, but also beneficial to the activation of the infrared reflective masterbatch, thereby improving the infrared reflection function.

[0011] Preferably, the upper coating layer includes infrared reflective masterbatch and at least one of low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), polyethylene (PE), and polypropylene (PP).

[0012] Preferably, in the infrared reflective masterbatch, the melt index of the low-density polyethylene (LDPE) is 1.5-4.5 g / 10 min (2160 g); further preferably, the melt index of the low-density polyethylene (LDPE) is 2-4 g / 10 min (2160 g).

[0013] Preferably, in the infrared reflective masterbatch, the melt index of the linear low-density polyethylene (LLDPE) is 6-9 g / 10 min (2160 g); further preferably, the melt index of the linear low-density polyethylene (LLDPE) is 7-9 g / 10 min (2160 g).

[0014] Preferably, the infrared reflective masterbatch comprises, by weight, 20-30 parts of nano-silicon dioxide-coated titanium dioxide and / or nano-zirconium oxide, 72 parts of low-density polyethylene (LDPE), and 8-12 parts of linear low-density polyethylene (LLDPE).

[0015] Preferably, the upper coating layer comprises, by weight, 40-60 parts of low-density polyethylene (LDPE), 20-40 parts of linear low-density polyethylene (LLDPE), and 10-20 parts of infrared reflective masterbatch; further preferably, the upper coating layer comprises, by weight, 40-50 parts of low-density polyethylene (LDPE), 35-40 parts of linear low-density polyethylene (LLDPE), and 15-20 parts of infrared reflective masterbatch.

[0016] Preferably, the lower coating layer, by weight, comprises 40-60 parts of low-density polyethylene (LDPE), 20-40 parts of linear low-density polyethylene (LLDPE), and 0-20 parts of infrared reflective masterbatch; further preferably, the upper coating layer, by weight, comprises 40-50 parts of low-density polyethylene (LDPE), 35-40 parts of linear low-density polyethylene (LLDPE), and 0-20 parts of infrared reflective masterbatch.

[0017] Preferably, in the upper coating layer, the melt index of the linear low-density polyethylene (LLDPE) is 3-5 g / 10 min (2160 g).

[0018] Preferably, the braided layer is woven from flat yarns, and the components of the flat yarns include high-density polyethylene (HDPE) and / or polypropylene (PP). That is, the flat yarns composed of high-density polyethylene (HDPE) and / or polypropylene (PP) are woven by a plastic circular loom or a flat loom.

[0019] Preferably, the weight per unit area of ​​the woven layer is 30-110 g / m 2 Further preferably, the weight per unit area of ​​the woven layer is 40-90g / m 2 .

[0020] Preferably, the weight per unit area of ​​the upper coating layer and the lower coating layer is 10-90 g / m 2 Further preferably, the weight per unit area of ​​the upper coating layer and the lower coating layer is 18-40g / m 2 .

[0021] A second aspect of the present invention provides a method for preparing a composite plastic woven cloth with infrared reflection function.

[0022] Specifically, a method for preparing a composite plastic woven fabric with infrared reflection function comprises the following steps:

[0023] (1) mixing nano-silicon dioxide-coated titanium dioxide and / or nano-zirconium dioxide, low-density polyethylene, and linear low-density polyethylene, and extruding and granulating to obtain the infrared reflective masterbatch;

[0024] (2) weaving the flat wire into a braided layer;

[0025] (3) Coating the components of the upper coating layer and the lower coating layer on the upper and lower surfaces of the woven layer to obtain the composite plastic woven fabric.

[0026] Preferably, in step (1), extrusion granulation is carried out in a twin-screw extruder.

[0027] Preferably, in step (2), high density polyethylene (HDPE) and / or polypropylene (PP) are used to prepare flat yarns by wire drawing, which is a conventional process in the art.

[0028] Preferably, in step (3), the components of the upper coating layer and the lower coating layer are first mixed in an extruder and then coated in a casting compounder.

[0029] A third aspect of the present invention provides an application of a composite plastic woven cloth with infrared reflection function.

[0030] The composite plastic woven fabric with infrared reflection function is used in agricultural greenhouses or waterproof rolls.

[0031] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0032] The composite plastic woven fabric of the present invention comprises, from bottom to top, a lower coating layer, a woven layer, and an upper coating layer in sequence; the upper coating layer comprises an infrared reflective masterbatch, and the infrared reflective masterbatch comprises nano-silicon dioxide-coated titanium dioxide and / or nano-zirconium oxide, low-density polyethylene, and linear low-density polyethylene; the infrared reflective masterbatch comprises 10-30 parts of nano-silicon dioxide-coated titanium dioxide and / or nano-zirconium oxide, 60-80 parts of low-density polyethylene (LDPE), and 4-12 parts of linear low-density polyethylene (LLDPE) by weight. The special components and content of the infrared reflective masterbatch enable the infrared reflective masterbatch to be added to the upper coating layer to interact with other components, thereby significantly improving the infrared reflective function and waterproof effect of the composite plastic woven fabric. For example, the reflectance ratio for near infrared exceeds 0.8. The woven layer provides strong structural support for the composite plastic woven fabric. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a schematic structural diagram of the composite plastic woven fabric prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0034] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.

[0035] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0036] The nano-silicon dioxide-coated titanium dioxide used in the following examples was provided by Jiangsu Panhua Chemical Technology Co., Ltd.

[0037] Nano-zirconia was provided by Jiangsu Xinxing Chemical Industry Group Co., Ltd.

[0038] Low-density polyethylene (LDPE) and linear low-density polyethylene (LLDPE) are provided by Sinopec or PetroChina.

[0039] Example 1

[0040] A composite plastic woven fabric with infrared reflection function, which comprises, from bottom to top, a lower coating layer, a woven layer, and an upper coating layer;

[0041] The upper coating layer includes infrared reflective masterbatch, which includes 20 parts of nano-silicon dioxide-coated titanium dioxide, 72 parts of low-density polyethylene (LDPE, model 2426H), 8 parts of linear low-density polyethylene (LLDPE, model 7144), and 5 parts of white mineral oil by weight;

[0042] In the infrared reflective masterbatch, the melt index of low-density polyethylene (LDPE) is 3g / 10min (2160g);

[0043] In the infrared reflective masterbatch, the melt index of linear low-density polyethylene (LLDPE) is 9 g / 10 min (2160 g);

[0044] The upper coating layer includes, by weight, 50 parts of low-density polyethylene (LDPE), 35 parts of linear low-density polyethylene (LLDPE), and 15 parts of infrared reflective masterbatch;

[0045] The lower coating layer includes, by weight, 50 parts of low-density polyethylene (LDPE), 35 parts of linear low-density polyethylene (LLDPE), and 15 parts of infrared reflective masterbatch;

[0046] In the upper coating layer and the lower coating layer, the melt index of the linear low-density polyethylene (LLDPE) is 4 g / 10 min (2160 g).

[0047] The braided layer is woven from flat wires, and the component of the flat wires is high-density polyethylene (HDPE);

[0048] The unit area weight of the woven layer is 80g / m 2 ;

[0049] The unit area weight of the upper and lower coating layers is 50g / m 2 .

[0050] Figure 1 This is a schematic structural diagram of the composite plastic woven fabric prepared in Example 1 of the present invention. Figure 1 100 represents the lower coating layer, 200 represents the woven layer, and 300 represents the upper coating layer.

[0051] A method for preparing a composite plastic woven cloth with infrared reflection function comprises the following steps:

[0052] (1) mixing nano-silica-coated titanium dioxide, low-density polyethylene, linear low-density polyethylene, and white mineral oil, and extruding and granulating the mixture in a twin-screw granulator (the temperature distribution of barrel 1, barrel 2, barrel 3, barrel 4, barrel 5, barrel 6, filter screen area, connector, and die head in the twin-screw granulator is: 180° C., 200° C., 210° C., 220° C., 220° C., 225° C., 230° C., 230° C., 220° C.), to obtain an infrared reflective masterbatch;

[0053] (2) using a conventional wire drawing method to make a flat wire from high-density polyethylene (HDPE), and weaving the flat wire into a braided layer using a plastic circular loom;

[0054] (3) The components of the upper coating layer and the lower coating layer are mixed in an extruder (the temperature distribution of barrel 1, barrel 2, barrel 3, barrel 4, barrel 5, barrel 6, filter area, connector, and die head in the extruder is: 180°C, 230°C, 250°C, 260°C, 260°C, 270°C, 270°C, 275°C, and 270°C), and then coated on the upper and lower surfaces of the woven layer in a cast-film composite machine, and cooled to room temperature to obtain a composite plastic woven fabric.

[0055] Example 2

[0056] A composite plastic woven fabric with infrared reflection function, which comprises, from bottom to top, a lower coating layer, a woven layer, and an upper coating layer;

[0057] The upper coating layer includes infrared reflective masterbatch, which includes 20 parts of nano zirconium oxide, 72 parts of low-density polyethylene (LDPE, model 2426H), 8 parts of linear low-density polyethylene (LLDPE, model 7144), and 2 parts of white mineral oil by weight;

[0058] In the infrared reflective masterbatch, the melt index of low-density polyethylene (LDPE) is 3g / 10min (2160g);

[0059] In the infrared reflective masterbatch, the melt index of linear low-density polyethylene (LLDPE) is 9 g / 10 min (2160 g);

[0060] The upper coating layer includes, by weight, 50 parts of low-density polyethylene (LDPE), 35 parts of linear low-density polyethylene (LLDPE), and 15 parts of infrared reflective masterbatch;

[0061] The lower coating layer includes, by weight, 50 parts of low-density polyethylene (LDPE), 35 parts of linear low-density polyethylene (LLDPE), and 15 parts of infrared reflective masterbatch;

[0062] In the upper coating layer and the lower coating layer, the melt index of the linear low-density polyethylene (LLDPE) is 4 g / 10 min (2160 g).

[0063] The braided layer is woven from flat wires, and the component of the flat wires is high-density polyethylene (HDPE);

[0064] The unit area weight of the woven layer is 80g / m 2 ;

[0065] The unit area weight of the upper and lower coating layers is 50g / m 2 .

[0066] A method for preparing a composite plastic woven cloth with infrared reflection function comprises the following steps:

[0067] (1) mixing nano zirconium oxide, low-density polyethylene, linear low-density polyethylene and white mineral oil, and extruding and granulating the mixture in a twin-screw granulator (the temperature distribution of barrel 1, barrel 2, barrel 3, barrel 4, barrel 5, barrel 6, filter screen area, connector and die head in the twin-screw granulator is 180° C., 200° C., 210° C., 220° C., 220° C., 225° C., 230° C., 230° C. and 220° C.) to obtain an infrared reflective masterbatch;

[0068] (2) using a conventional wire drawing method to make a flat wire from high-density polyethylene (HDPE), and weaving the flat wire into a braided layer using a plastic circular loom;

[0069] (3) The components of the upper coating layer and the lower coating layer are mixed in an extruder (the temperature distribution of barrel 1, barrel 2, barrel 3, barrel 4, barrel 5, barrel 6, filter area, connector, and die head in the extruder is: 180°C, 230°C, 250°C, 260°C, 260°C, 270°C, 270°C, 275°C, and 270°C), and then coated on the upper and lower surfaces of the woven layer in a cast-film composite machine, and cooled to room temperature to obtain a composite plastic woven fabric.

[0070] Comparative Example 1

[0071] Compared with Example 1, the difference of Comparative Example 1 is that the nano-silicon dioxide-coated titanium dioxide in Example 1 is replaced by an equal amount of rutile titanium dioxide, and the rest of the process is the same as that of Example 1.

[0072] Comparative Example 2

[0073] Compared with Example 1, the difference of Comparative Example 2 is that in the infrared reflective masterbatch and the upper coating layer, an equal amount of linear low-density polyethylene is used to replace the low-density polyethylene in Example 1, and the rest of the process is the same as Example 1.

[0074] Product effect testing

[0075] The composite plastic woven fabric (film thickness is about 60 μm) prepared in Examples 1-2 and Comparative Example 1 was taken, and the brightness of the composite plastic woven fabric was tested according to standard GB / T11186.2, and the solar reflectance and near-infrared reflectance of the composite plastic woven fabric were tested according to JG / T235-2014. The results are shown in Table 1.

[0076] Table 1

[0077] Lightness (L*) Solar reflectance Near infrared reflectance Example 1 98.313 0.881 0.881 Example 2 92.920 0.836 0.811 Comparative Example 1 97.731 0.804 0.641

[0078] It can be seen from Table 1 that the infrared reflection effect of the composite plastic woven fabric prepared by the present invention is obviously better than that of Comparative Example 1.

[0079] In addition, the waterproof performance of the composite plastic woven fabrics prepared in the above-mentioned Example 1 and Comparative Example 2 was also tested. The specific process is to place the composite plastic woven fabrics prepared in the above-mentioned Example 1 and Comparative Example 2 under a water pressure of 0.7 MPa, and observe whether water passes through the composite plastic woven fabric after 30 minutes. The results show that no water passes through the composite plastic woven fabric prepared in Example 1, while a small amount of water passes through Comparative Example 2. From this courseware, the appropriate amount of each component has a significant effect on the waterproof performance of the composite plastic woven fabric.

Claims

1. A composite plastic woven fabric, characterized in that: From bottom to top, it includes lower coating layer, woven layer and upper coating layer; The upper coating layer comprises an infrared reflective masterbatch, which comprises, by weight, 10-30 parts of nano-silicon dioxide-coated titanium dioxide and / or nano-zirconium oxide, 60-80 parts of low-density polyethylene, and 4-12 parts of linear low-density polyethylene; The upper coating layer comprises, by weight, 40-60 parts of low-density polyethylene, 20-40 parts of linear low-density polyethylene, and 10-20 parts of infrared reflective masterbatch; The lower coating layer comprises, by weight, 40-60 parts of low-density polyethylene, 20-40 parts of linear low-density polyethylene, and 0-20 parts of infrared reflective masterbatch.

2. The composite plastic woven fabric according to claim 1, characterized in that: The braided layer is braided from flat wires, and the components of the flat wires include high-density polyethylene and / or polypropylene.

3. The composite plastic woven fabric according to claim 1, characterized in that: The unit area weight of the braided layer is 30-110 g / m 2 .

4. The composite plastic woven fabric according to claim 1, characterized in that: The unit area weight of the upper coating layer and the lower coating layer is 10-90g / m 2 .

5. The method for preparing the composite plastic woven fabric according to any one of claims 1 to 4, characterized in that: The following steps are involved: (1) mixing nano-silicon dioxide-coated titanium dioxide and / or nano-zirconium dioxide, low-density polyethylene, and linear low-density polyethylene, and extruding and granulating to obtain the infrared reflective masterbatch; (2) weaving the flat wire into a braided layer; (3) Coating the components of the upper coating layer and the lower coating layer on the upper and lower surfaces of the woven layer to obtain the composite plastic woven fabric.

6. The preparation method according to claim 5, characterized in that: In step (3), the components of the upper coating layer and the lower coating layer are firstly mixed in an extruder and then coated in a casting compounder.

7. Use of the composite plastic woven fabric according to any one of claims 1 to 4 in agricultural greenhouses or waterproof rolls.

Citation Information

Patent Citations

  • Infrared reflective film, infrared reflective paint, and infrared reflector

    CN104024352A

  • High-weatherability white ASA resin applied to extrusion molding and preparation method thereof

    CN104004310A

  • Polyethylene plastic greenhouse cloth and preparation method thereof

    CN109371700A

  • Breathable reflective lawn-proof cloth and preparation method thereof

    CN110607699A

  • Triplelayer polyethylene heat shrinkable film

    KR101317856B1