High frequency dielectric heating adhesive sheet, bonding method and bonding body
By using reactive thermoplastic resin, dielectric material and silane coupling agent in the adhesive layer, combined with high-frequency electric field technology, the problem of insufficient bonding strength of glass materials in the prior art is solved, and high-frequency dielectric heating adhesive is achieved The high bonding strength of the joints is effective bonded to the glass.
Patent Information
- Application Number
- CN202180047061.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-06-30
- Filing Date
- 2021-06-25
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-06-25
AI Technical Summary
It is difficult to obtain sufficient bonding with high bond strength to glass materials in the prior art, especially in dielectric heating adhesive films.
The adhesive sheet is adopted with a high-frequency dielectric heating adhesive sheet, and the adhesive layer contains a thermoplastic resin in the reactive part, a dielectric material that generates heat through a high-frequency electric field, and a silane coupling agent. The volume content of the silane coupling agent is more than 0.5% and The volume average particle size of the dielectric filler is 1 μm or more and 30 μm or less.
It is possible to achieve high bonding strength and glass bonding even with less energy consumption, and improve the bonding strength and durability of the glass-based adherents.
Smart Images

Figure CN115812092B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a high-frequency dielectric heating adhesive sheet, a joining method and a joined body. Background Art
[0002] In recent years, as a method for bonding adherends that are usually difficult to bond, methods such as sandwiching an adhesive made of a heat-generating material blended in a given resin between the adherends and performing dielectric heating treatment, induction heating treatment, ultrasonic welding treatment, or laser welding treatment have been proposed.
[0003] As a bonding method when using glass as an adherend, there are the following techniques.
[0004] For example, Patent Document 1 describes a dielectric heating adhesive film for bonding a plurality of adherends formed of the same material or different materials. The dielectric heating adhesive film includes a polyolefin resin having a polar portion and a dielectric filler blended in a predetermined ratio.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. 2018 / 147352 Summary of the invention
[0008] Problem that the invention aims to solve
[0009] Although Patent Document 1 also describes a glass material as an example of an adherend, it is difficult for the dielectric heating adhesive film described in Patent Document 1 to obtain sufficient bonding strength to the glass material.
[0010] The object of the present invention is to provide a high-frequency dielectric heating adhesive sheet that can be bonded to glass with high bonding strength even with low energy consumption, to provide a joining method using the high-frequency dielectric heating adhesive sheet, and to provide a joined body formed by joining glass adherends with high bonding strength.
[0011] Solutions to the problem
[0012] According to one embodiment of the present invention, there is provided a high-frequency dielectric heating adhesive sheet having an adhesive layer containing a thermoplastic resin (A) having a reactive site (Y), a dielectric material that generates heat when a high-frequency electric field is applied, and a silane coupling agent (C).
[0013] In the high-frequency dielectric heating adhesive sheet according to one embodiment of the present invention, the volume content of the silane coupling agent (C) in the adhesive layer is preferably 0.5% by volume or more and 25% by volume or less.
[0014] In the high-frequency dielectric heating adhesive sheet of one embodiment of the present invention, the silane coupling agent (C) preferably contains a functional group (X) and an alkoxysilyl group (Z), and the number of atoms of the main chain connecting the functional group (X) and the silicon atom of the alkoxysilyl group (Z) is 6 or more.
[0015] In the high-frequency dielectric heating adhesive sheet according to one embodiment of the present invention, it is preferred that the molecular weight of the silane coupling agent (C) is 200 or more.
[0016] In the high-frequency dielectric heating adhesive sheet according to one embodiment of the present invention, it is preferred that the functional group (X) is at least one group selected from the group consisting of an epoxy group, an amino group, an isocyanate group, and a mercapto group.
[0017] In the high-frequency dielectric heating adhesive sheet of one embodiment of the present invention, the difference ΔT between the 5% weight loss temperature Td5 of the silane coupling agent (C) represented by the following mathematical formula (Math. 1) and the flow starting temperature Tfs of the thermoplastic resin (A) is preferably -20°C or more.
[0018] ΔT=Td5-Tfs…(Formula 1)
[0019] In the high-frequency dielectric heating adhesive sheet according to one embodiment of the present invention, it is preferred that the silane coupling agent (C) has a 5% weight loss temperature of 120° C. or higher.
[0020] In the high-frequency dielectric heating adhesive sheet according to one embodiment of the present invention, it is preferred that the reactive site (Y) includes at least one selected from a carboxyl group, a hydroxyl group, an amino group, an isocyanate group, and an acid anhydride structure.
[0021] In the high-frequency dielectric heating adhesive sheet according to one embodiment of the present invention, it is preferred that the reactive site (Y) include a maleic anhydride structure.
[0022] In the high-frequency dielectric heating adhesive sheet according to one embodiment of the present invention, it is preferred that the thermoplastic resin (A) is a polyolefin-based resin.
[0023] In the high-frequency dielectric heating adhesive sheet according to one embodiment of the present invention, it is preferred that the volume content of the dielectric material in the adhesive layer is 5 volume % or more and 50 volume % or less.
[0024] In the high-frequency dielectric heating adhesive sheet according to one embodiment of the present invention, it is preferred that the dielectric material is a dielectric filler (B).
[0025] In the high-frequency dielectric heating adhesive sheet according to one embodiment of the present invention, it is preferred that the dielectric filler (B) includes at least one selected from the group consisting of zinc oxide, silicon carbide, barium titanate, and titanium oxide.
[0026] In one embodiment of the high-frequency dielectric heating adhesive sheet of the present invention, the volume average particle size of the dielectric filler (B) is preferably 1 μm or more and 30 μm or less. The volume average particle size is the volume average particle size calculated based on the particle size distribution measured by laser diffraction / scattering method and JIS Z 8819-2:2001.
[0027] According to one embodiment of the present invention, a joining method can be provided, which includes: a process of configuring a high-frequency dielectric heating adhesive sheet of one embodiment of the present invention between a first adherend and a second adherend; and a process of applying a high-frequency electric field to the above-mentioned high-frequency dielectric heating adhesive sheet to join the above-mentioned first adherend and the above-mentioned second adherend.
[0028] According to one embodiment of the present invention, a bonding sheet can be provided, which has a first adherend, a second adherend, and a high-frequency dielectric heating adhesive sheet of one embodiment of the present invention, wherein at least any one of the above-mentioned first adherend and the above-mentioned second adherend is a glass adherend, and the above-mentioned first adherend and the above-mentioned second adherend are bonded together by the above-mentioned high-frequency dielectric heating adhesive sheet.
[0029] According to one embodiment of the present invention, a high-frequency dielectric heating adhesive sheet can be provided that can be bonded to glass with high bonding strength even with low energy consumption. According to one embodiment of the present invention, a bonding method using the high-frequency dielectric heating adhesive sheet can be provided. According to one embodiment of the present invention, a bonded body formed by bonding glass adherends with high bonding strength can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1A The diagram is a cross-sectional view of a high-frequency dielectric heating adhesive sheet according to an embodiment.
[0031] Figure 1B The diagram is a cross-sectional view of a high-frequency dielectric heating adhesive sheet according to an embodiment.
[0032] Figure 1C The diagram is a cross-sectional view of a high-frequency dielectric heating adhesive sheet according to an embodiment.
[0033] Figure 2 This is a schematic diagram for explaining a high-frequency dielectric heating process using a high-frequency dielectric heating adhesive sheet and a dielectric heating device according to one embodiment.
[0034] Explanation of symbols
[0035] 10…adhesive layer (first adhesive layer), 11…first surface, 12…second surface, 110…first adherend, 120…second adherend, 1A…high-frequency dielectric heating adhesive sheet, 1B…high-frequency dielectric heating adhesive sheet, 1C…high-frequency dielectric heating adhesive sheet, 20…adhesive layer (second adhesive layer), 21…second surface, 30…substrate, 40…intermediate layer, 50…dielectric heating adhesive device, 51…first high-frequency electric field applying electrode, 52…second high-frequency electric field applying electrode, 53…high-frequency power supply. DETAILED DESCRIPTION
[0036] [High frequency dielectric heating adhesive sheet]
[0037] The high-frequency dielectric heating adhesive sheet of this embodiment has an adhesive layer containing a thermoplastic resin (A) having a reactive site (Y), a dielectric material that generates heat when a high-frequency electric field is applied, and a silane coupling agent (C). The high-frequency electric field is an electric field that reverses direction at high frequencies.
[0038] The dielectric material is a material that generates heat by applying a high-frequency electric field, and is preferably a material that generates heat when a high-frequency electric field with a frequency range of 3 MHz or more and 300 MHz or less is applied. The dielectric material is preferably at least one of a dielectric resin and a dielectric filler. From the viewpoint of easily suppressing the degradation of the dielectric material contained in the high-frequency dielectric heating adhesive sheet when processing the high-frequency dielectric heating adhesive sheet, the dielectric material is more preferably a dielectric filler (B).
[0039] Hereinafter, a case where the high-frequency dielectric heating adhesive sheet of the present embodiment includes a dielectric filler (B) as a dielectric material will be described.
[0040] <Thermoplastic Resin (A) Having Reactive Site (Y)>
[0041] The thermoplastic resin (A) has at least one reactive site (Y). When the thermoplastic resin (A) has two or more reactive sites (Y), the two or more reactive sites (Y) may be the same or different from each other.
[0042] Examples of the reactive site (Y) of the thermoplastic resin (A) include a carboxyl group, a hydroxyl group, an amino group, an isocyanate group, an epoxy group, a vinyl acetate structure, and an acid anhydride structure. The reactive site (Y) can be introduced by copolymerization with the thermoplastic resin or by graft modification.
[0043] Since the thermoplastic resin (A) has at least one reactive site (Y), the silane coupling agent acts on both the reactive site (Y) of the thermoplastic resin and the glass as the adherend, so that the adhesive layer of the high-frequency dielectric heating adhesive sheet can easily and firmly bond to the adherend.
[0044] The reactive part (Y) of the thermoplastic resin (A) preferably includes at least one selected from a carboxyl group, a hydroxyl group, an amino group, an isocyanate group, and an acid anhydride structure, and more preferably includes at least one selected from a carboxyl group and an acid anhydride structure. By making the reactive part (Y) of the thermoplastic resin (A) include at least one of a carboxyl group and an acid anhydride structure, the adhesive layer of the high-frequency dielectric heating adhesive sheet has excellent adhesion and time stability.
[0045] Examples of the compound used when introducing the reactive site (Y) into the thermoplastic resin include unsaturated carboxylic acid derivative components derived from any of unsaturated carboxylic acids, anhydrides of unsaturated carboxylic acids, and esters of unsaturated carboxylic acids.
[0046] As unsaturated carboxylic acid, acrylic acid, methacrylic acid, maleic acid, fumaric acid, itaconic acid, citraconic acid, etc. are mentioned, for example.
[0047] As an anhydride of an unsaturated carboxylic acid, anhydrides of unsaturated carboxylic acids, such as maleic anhydride, itaconic anhydride and citraconic anhydride, etc. are mentioned, for example.
[0048] Examples of the ester of unsaturated carboxylic acid include esters of unsaturated carboxylic acids such as methyl acrylate, ethyl acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, dimethyl maleate, monomethyl maleate, dimethyl fumarate, diethyl fumarate, dimethyl itaconate, diethyl itaconate, dimethyl citrate, diethyl citrate, and dimethyl tetrahydrophthalate.
[0049] Hereinafter, the thermoplastic resin (A) having a reactive site (Y) is referred to as a thermoplastic resin (A).
[0050] The reactive part (Y) of the thermoplastic resin (A) preferably comprises a maleic anhydride structure. The maleic anhydride structure may be a group introduced by grafting and modifying the thermoplastic resin. In addition, the thermoplastic resin (A) may also be a maleic anhydride copolymer obtained by copolymerizing a monomer comprising a maleic anhydride structure. The reactive part (Y) may be a structure derived from maleic anhydride in the maleic anhydride copolymer.
[0051] When the thermoplastic resin (A) contains a maleic anhydride structure as the reactive site (Y), the reactive site (Y) easily reacts with the functional group (X) of the silane coupling agent (C). Therefore, when the thermoplastic resin (A) contains a maleic anhydride structure as the reactive site (Y), it is easy to bond the adherend more firmly.
[0052] As for the thermoplastic resin (A), from the viewpoint of being easy to melt and having a given heat resistance, it is preferably at least one selected from polyolefin resins, styrene resins, polyacetal resins, polycarbonate resins, polyacrylic resins, polyamide resins, polyimide resins, polyvinyl acetate resins, phenoxy resins and polyester resins, and more preferably a polyolefin resin.
[0053] Polyolefin resins are inexpensive but have excellent moldability and mechanical strength.
[0054] (Polyolefin resin)
[0055] Examples of polyolefin resins as thermoplastic resins include resins formed from homopolymers such as polyethylene, polypropylene, polybutene, and polymethylpentene, and α-olefin resins formed from copolymers of monomers selected from ethylene, propylene, butene, hexene, octene, and 4-methylpentene, etc. The polyolefin resins as thermoplastic resins may be a single resin or a combination of two or more resins.
[0056] From the viewpoint of excellent mechanical strength and obtaining stable adhesive properties, the olefin-based monomer is preferably at least one of ethylene and propylene.
[0057] (Polyolefin resin having reactive site (Y))
[0058] When the polyolefin resin as the thermoplastic resin (A) is a copolymer of an olefin monomer and a monomer having a reactive site (Y), the copolymer preferably contains 2% by mass or more of a structural unit derived from a monomer having a reactive site (Y), more preferably 4% by mass or more, further preferably 5% by mass or more, and further preferably 6% by mass or more. In addition, the copolymer preferably contains 30% by mass or less of a structural unit derived from a monomer having a reactive site (Y), more preferably 25% by mass or less, further preferably 20% by mass or less, and further preferably 15% by mass or less.
[0059] By making the copolymer contain more than 2% by mass of structural units derived from monomers having a reactive site (Y), the bonding strength of the high-frequency dielectric heating adhesive sheet is improved. In addition, by making the copolymer contain less than 30% by mass of structural units derived from monomers having a reactive site (Y), the viscosity of the thermoplastic resin (A) can be suppressed from becoming too strong. As a result, it is easy to prevent the molding process of the high-frequency dielectric heating adhesive sheet from becoming difficult.
[0060] When the polyolefin resin as the thermoplastic resin (A) is graft-modified to introduce a reactive site (Y), the modification rate based on the reactive site (Y) is preferably 0.01 mass % or more, more preferably 0.1 mass % or more, and further preferably 0.2 mass % or more.
[0061] When the polyolefin resin as the thermoplastic resin (A) is subjected to graft modification to introduce a reactive site (Y), the modification rate based on the reactive site (Y) is preferably 30% by mass or less, more preferably 20% by mass or less, and further preferably 10% by mass or less.
[0062] In the case where a reactive part (Y) is introduced into a polyolefin resin as a thermoplastic resin (A) by graft modification, the bonding strength of the high-frequency dielectric heating adhesive sheet is improved by making the modification rate based on the reactive part (Y) 0.01% by mass or more. In addition, by making the modification rate based on the reactive part (Y) 30% by mass or less, the viscosity of the thermoplastic resin (A) can be suppressed from becoming too strong. As a result, it is easy to prevent the molding process of the high-frequency dielectric heating adhesive sheet from becoming difficult.
[0063] In the present specification, the modification ratio based on the reactive site (Y) is the percentage of the mass of the portion derived from the reactive site relative to the total mass of the polyolefin having the reactive site (Y).
[0064] In the polyolefin resin as the thermoplastic resin (A), the reactive site (Y) preferably has at least one selected from a carboxyl group, a hydroxyl group, an amino group, an isocyanate group and an acid anhydride structure, and more preferably has at least one of a carboxyl group and an acid anhydride structure. The acid anhydride structure is more preferably a maleic anhydride structure.
[0065] (Polyolefin having maleic anhydride structure)
[0066] When the polyolefin having a maleic anhydride structure is a copolymer of an olefin monomer and a monomer containing a maleic anhydride structure, the ratio of the structural unit derived from the monomer containing a maleic anhydride structure in the copolymer is preferably in the same range as the ratio of the structural unit derived from the monomer having a reactive site (Y) in the case of a copolymer of an olefin monomer and a monomer having a reactive site (Y). The effect obtained by being within this range is also the same as in the case where the polyolefin resin as the thermoplastic resin (A) is a copolymer with a monomer having a reactive site (Y).
[0067] In the polyolefin having a maleic anhydride structure, the modification ratio in the case of introducing the maleic anhydride structure by graft modification is preferably in the same range as the modification ratio in the case of introducing the reactive site (Y) by graft modification of the polyolefin resin as the thermoplastic resin (A). The effect obtained within this range is also the same as the case of introducing the reactive site (Y) by graft modification of the polyolefin resin as the thermoplastic resin (A).
[0068] The structural unit derived from olefin in the polyolefin having a maleic anhydride structure is preferably a structural unit derived from ethylene or propylene. That is, the polyolefin having a maleic anhydride structure is preferably a polyethylene resin having a maleic anhydride structure or a polypropylene resin having a maleic anhydride structure.
[0069] The flow initiation temperature of the thermoplastic resin (A) is preferably 80°C or higher, more preferably 85°C or higher, further preferably 90°C or higher, particularly preferably 95°C or higher.
[0070] The flow initiation temperature of the thermoplastic resin (A) is preferably 300°C or lower, more preferably 250°C or lower, and even more preferably 200°C or lower.
[0071] When the flow starting temperature of the thermoplastic resin (A) is 80° C. or higher, the adhesive layer tends to have good heat resistance.
[0072] When the flow initiation temperature of the thermoplastic resin (A) is 300° C. or lower, the adhesive layer can easily obtain good adhesiveness in a short time.
[0073] The flow initiation temperature of the adhesive layer can be measured by the method described in the section of Examples described later.
[0074] <Dielectric filler (B)>
[0075] The dielectric filler (B) is a filler that generates heat by application of a high-frequency electric field.
[0076] The dielectric filler (B) is preferably a filler that generates heat when a high-frequency electric field in the frequency range of 3 MHz to 300 MHz is applied. The dielectric filler (B) is preferably a filler that generates heat when a high-frequency electric field in the frequency range of 3 MHz to 300 MHz is applied, for example, a frequency of 13.56 MHz, 27.12 MHz, or 40.68 MHz.
[0077] (type)
[0078] The dielectric filler (B) is suitably one of the following materials alone or in combination of two or more thereof: zinc oxide, silicon carbide (SiC), anatase titanium oxide, barium titanate, barium zirconate titanate, lead titanate, potassium niobate, rutile titanium oxide, hydrated aluminum silicate, inorganic materials having water of crystallization such as hydrated aluminum silicates of alkali metals, or inorganic materials having water of crystallization such as hydrated aluminum silicates of alkaline earth metals.
[0079] The dielectric filler (B) preferably includes at least one selected from zinc oxide, silicon carbide, barium titanate, and titanium oxide.
[0080] Among the dielectric fillers exemplified, due to the rich variety, various shapes and sizes that can be selected, and the ability to improve the bonding properties and mechanical properties of the high-frequency dielectric heating adhesive sheet in accordance with the purpose, the dielectric filler (B) is further preferably zinc oxide. By using zinc oxide as a dielectric filler (B), a colorless high-frequency dielectric heating adhesive sheet can be obtained. Among dielectric fillers, the density of zinc oxide is small, so when a high-frequency dielectric heating adhesive sheet containing zinc oxide as a dielectric filler (B) is used to join the adherend, the total weight of the joint is not easy to increase compared to the case where a sheet containing other dielectric fillers is used. Zinc oxide has a low hardness in ceramics, so it is not easy to damage the manufacturing device of the high-frequency dielectric heating adhesive sheet. Since zinc oxide is an inactive oxide, even if it is combined with a thermoplastic resin, the damage caused to the thermoplastic resin is small.
[0081] The titanium oxide as the dielectric filler (B) is preferably at least one of anatase titanium oxide and rutile titanium oxide, and is more preferably anatase titanium oxide from the viewpoint of excellent dielectric properties.
[0082] (Volume content)
[0083] The volume content of the dielectric filler (B) in the adhesive layer is preferably 5 volume % or more, more preferably 8 volume % or more, and even more preferably 10 volume % or more.
[0084] The volume content of the dielectric filler (B) in the adhesive layer is preferably 50 volume % or less, more preferably 40 volume % or less, further preferably 35 volume % or less, and further preferably 25 volume % or less.
[0085] When the volume content of the dielectric filler (B) in the adhesive layer is 5 volume % or more, the heat generation property is improved, and the adhesive layer and the adherend made of glass can be easily firmly bonded.
[0086] When the volume content of the dielectric filler (B) in the adhesive layer is 50 volume % or less, flexibility when formed into a sheet can be easily obtained and a decrease in toughness can be easily prevented. Therefore, the high-frequency dielectric heating adhesive sheet can be easily processed into a desired shape in a subsequent step.
[0087] It should be noted that, in the high-frequency dielectric heating adhesive sheet of the present embodiment, since a thermoplastic resin (A), a dielectric filler (B) and a silane coupling agent (C) are included, the volume content of the dielectric filler (B) is preferably 5% by volume or more, more preferably 8% by volume or more, and further preferably 10% by volume or more relative to the total volume of the thermoplastic resin (A), the dielectric filler (B) and the silane coupling agent (C). The volume content of the dielectric filler (B) is preferably 50% by volume or less, more preferably 40% by volume or less, further preferably 35% by volume or less, and further preferably 25% by volume or less relative to the total volume of the thermoplastic resin (A), the dielectric filler (B) and the silane coupling agent (C).
[0088] In the above, as the volume content of the dielectric material in the adhesive layer, the volume content in the case where the dielectric material is the dielectric filler (B) is described. However, the volume content of the dielectric material in the adhesive layer is not limited to the case where the dielectric material is the dielectric filler (B), and in the case of a dielectric material other than the dielectric filler (B), it is also suitable to be in the same range as the volume content of the dielectric filler (B) in the adhesive layer. That is, the volume content of the dielectric material in the adhesive layer is preferably 5 volume % or more and preferably 50 volume % or less.
[0089] (Average particle size)
[0090] The volume average particle size of the dielectric filler (B) is preferably 1 μm or more, more preferably 2 μm or more, and even more preferably 3 μm or more.
[0091] The volume average particle size of the dielectric filler (B) is preferably 30 μm or less, more preferably 25 μm or less, and even more preferably 20 μm or less.
[0092] When the volume average particle size of the dielectric filler (B) is 1 μm or more, the high-frequency dielectric heating adhesive sheet exhibits high heat generation performance when a high-frequency electric field is applied, and the adhesive layer can be strongly bonded to a glass adherend in a short time.
[0093] By making the volume average particle size of the dielectric filler (B) less than 30 μm, the high-frequency dielectric heating adhesive sheet will show high heat generation performance when a high-frequency electric field is applied, and the adhesive layer can be strongly bonded to the glass adherend in a short time. In addition, by making the volume average particle size of the dielectric filler (B) less than 30 μm, the strength of the high-frequency dielectric heating adhesive sheet can be prevented from decreasing.
[0094] The volume average particle size of the dielectric filler (B) can be measured by the following method: The particle size distribution of the dielectric filler (B) is measured by laser diffraction / scattering method, and the volume average particle size is calculated based on the results of the particle size distribution measurement in accordance with JIS Z 8819-2:2001.
[0095] In the high-frequency dielectric heating adhesive sheet of this embodiment, it is preferred that the average particle size D of the dielectric filler (B) is F The thickness T of the bonding layer satisfies 1≤T / D F Relationship ≤2500.
[0096] T / D F It is preferably 1 or more, preferably 2 or more, preferably 5 or more, more preferably 10 or more, and further preferably 20 or more. T / D F When the ratio is 1 or more, it is possible to prevent a decrease in bonding strength due to contact between the dielectric filler (B) and the adherend during bonding.
[0097] T / D F It is preferably 2500 or less, preferably 2000 or less, preferably 1750 or less, more preferably 1000 or less, further preferably 500 or less, further preferably 100 or less, and further more preferably 50 or less. T / D F When the molecular weight is 2500 or less, the burden on the sheet manufacturing apparatus when producing the high-frequency dielectric heating adhesive sheet can be suppressed.
[0098] <Silane coupling agent (C)>
[0099] The volume content of the silane coupling agent (C) in the adhesive layer is preferably 0.5 volume % or more, more preferably 1 volume % or more, further preferably 3 volume % or more, and further preferably 5 volume % or more.
[0100] The volume content of the silane coupling agent (C) in the adhesive layer is preferably 25 volume % or less, more preferably 20 volume % or less, further preferably 15 volume % or less, further preferably 12 volume % or less, and further preferably 10 volume % or less.
[0101] When the volume content of the silane coupling agent (C) in the adhesive layer is 0.5 volume % or more, it is easy to strongly bond the adhesive layer to a glass adherend.
[0102] When the volume content of the silane coupling agent (C) in the adhesive layer is 25 volume % or less, adhesive strength can be easily obtained.
[0103] When the volume content of the silane coupling agent (C) in the adhesive layer is 10 volume % or less, it is easy to suppress the bleed-out of the silane coupling agent (C) from the adhesive layer.
[0104] As the silane coupling agent (C), a known silane coupling agent can be used. The silane coupling agent (C) is preferably an organic silicon compound having at least one alkoxysilyl group in the molecule.
[0105] Examples of the silane coupling agent include silane coupling agents having a (meth)acryloyl group, such as 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, and 8-methacryloxyoctyltrimethoxysilane; vinyltrimethoxysilane, vinyltriethoxysilane, dimethoxymethylvinylsilane, diethoxymethylvinylsilane, trichlorovinylsilane, vinyltri(2-methoxyethoxy)silane, and 6-octenyltrimethoxysilane. Silane coupling agents having vinyl groups, such as silane; 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, and 8-glycidoxyoctyltrimethoxysilane; silane coupling agents having styrene groups, such as p-phenylethylenetrimethoxysilane and p-phenylethylenetriethoxysilane; N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyl Silane coupling agents having an amino group such as triethoxysilane, N-2-(aminoethyl)-8-aminooctyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, and N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane hydrochloride; silane coupling agents having a urea group such as 3-ureidopropyltrimethoxysilane and 3-ureidopropyltriethoxysilane; silane coupling agents having a halogen atom such as 3-chloropropyltrimethoxysilane and 3-chloropropyltriethoxysilane Silane coupling agents having a mercapto group, such as 3-mercaptopropylmethyldimethoxysilane and 3-mercaptopropyltrimethoxysilane; silane coupling agents having a sulfide group, such as bis(trimethoxysilylpropyl)tetrasulfide and bis(triethoxysilylpropyl)tetrasulfide; silane coupling agents having an isocyanate group, such as 3-isocyanatepropyltrimethoxysilane and 3-isocyanatepropyltriethoxysilane; silane coupling agents having an allyl group, such as allyltrichlorosilane, allyltriethoxysilane and allyltrimethoxysilane; silane coupling agents having a hydroxyl group, such as 3-hydroxypropyltrimethoxysilane and 3-hydroxypropyltriethoxysilane; etc. It should be noted that in this specification, "(meth)acryloyl" is the recording method used when indicating both "acryloyl" and "methacryloyl", and the same applies to other similar terms.
[0106] The silane coupling agent (C) preferably contains a functional group (X) and an alkoxysilyl group (Z).
[0107] The number of atoms in the main chain linking the functional group (X) and the silicon atom of the alkoxysilyl group (Z) is preferably 6 or more, more preferably 8 or more.
[0108] The number of atoms in the main chain linking the functional group (X) and the silicon atom of the alkoxysilyl group (Z) is preferably 50 or less, more preferably 30 or less, further preferably 20 or less, and further preferably 15 or less.
[0109] The number of atoms in the main chain connecting the functional group (X) and the silicon atom of the alkoxysilyl group (Z) is the number of atoms on the main chain, and does not include the number of side chains, hydrogen atoms, and atoms other than hydrogen atoms (for example, when the main chain contains a ketone, the number of oxygen atoms bonded to the carbon atom of the ketone) bonded to the atoms constituting the main chain.
[0110] When the number of atoms of the main chain linking the functional group (X) and the silicon atom of the alkoxysilyl group (Z) is 6 or more, the silane coupling agent (C) is less likely to volatilize during melt kneading of the adhesive layer material, and the amount of the silane coupling agent added in the adhesive layer can be easily controlled.
[0111] When the number of atoms of the main chain linking the functional group (X) and the silicon atom of the alkoxysilyl group (Z) is 50 or less, it is easy to suppress a decrease in the reactivity between the reactive site (Y) of the thermoplastic resin (A) and the functional group (X) of the silane coupling agent (C).
[0112] For example, in the case of 8-glycidoxyoctyltrimethoxysilane, the number of atoms in the main chain linking the functional group (X) and the silicon atom of the alkoxysilyl group (Z) is 10 as shown below.
[0113] [Chemical formula 1]
[0114]
[0115] For example, in the case of N-2-(aminoethyl)-8-aminooctyltrimethoxysilane, the number of atoms in the main chain linking the functional group (X) and the silicon atom of the alkoxysilyl group (Z) is 11 as shown below.
[0116] [Chemical formula 2]
[0117]
[0118] In addition, the functional group (X) of the silane coupling agent (C) is a functional group bonded to the end of the main chain bonded to the silicon atom of the alkoxysilyl group (Z). For example, in the case of 8-glycidoxyoctyltrimethoxysilane, the epoxy group bonded to the end of the main chain is the functional group (X), and the ether bond in the main chain is not included in the functional group (X). In addition, for example, in the case of N-2-(aminoethyl)-8-aminooctyltrimethoxysilane, the amino group (-NH2) bonded to the end of the main chain is the functional group (X), and the amino group (-NH-) in the main chain is not included in the functional group (X). In addition, when the chain bonded to the silicon atom of the alkoxysilyl group (Z) contains a plurality of side chains having the functional group (X) at the end, the plurality of functional groups (X) in the silane coupling agent (C) are the same or different from each other. When a plurality of branch chains having a functional group (X) are included at the terminal, the main chain is a chain having the largest number of atoms linking the functional group (X) and the silicon atom of the alkoxysilyl group (Z).
[0119] The functional group (X) is preferably at least one group selected from an epoxy group, an amino group, an isocyanate group and a mercapto group, and more preferably at least one group selected from an epoxy group and an amino group. Since the epoxy group and the amino group as the functional group (X) are easy to react with the reactive site (Y) of the thermoplastic resin (A), it is easy to suppress the silane coupling agent (C) from seeping out of the adhesive layer. In the case where the silane coupling agent (C) has an epoxy group and an amino group as the functional group (X), the reactive site (Y) of the thermoplastic resin (A) is preferably a maleic anhydride structure.
[0120] The silane coupling agent (C) is preferably at least one of 8-glycidoxyoctyltrimethoxysilane and 3-glycidoxypropyltrimethoxysilane.
[0121] From the viewpoint of process suitability when producing an adhesive sheet, 8-glycidoxyoctyltrimethoxysilane is preferred, and from the viewpoint of economic efficiency, 3-glycidoxypropyltrimethoxysilane is preferred.
[0122] The adhesive sheet may contain a single silane coupling agent (C) or may contain two or more silane coupling agents (C).
[0123] The molecular weight of the silane coupling agent (C) is preferably 200 or more, more preferably 225 or more, further preferably 250 or more, and further preferably 280 or more.
[0124] The molecular weight of the silane coupling agent (C) is preferably 1,000 or less, more preferably 600 or less, further preferably 500 or less, and further preferably 400 or less.
[0125] By setting the molecular weight of the silane coupling agent (C) to be 200 or more, it is easy to prevent an undesirable reaction during processing.
[0126] When the molecular weight of the silane coupling agent (C) is 250 or more, the silane coupling agent (C) is less likely to volatilize during melt-kneading of the adhesive layer material, and the amount of the silane coupling agent added to the adhesive layer can be easily controlled.
[0127] By setting the molecular weight of the silane coupling agent (C) to be 1,000 or less, it is easy to suppress a decrease in the reactivity between the reactive site (Y) of the thermoplastic resin (A) and the functional group (X) of the silane coupling agent (C).
[0128] The difference ΔT between the 5% weight loss temperature Td5 of the silane coupling agent (C) represented by the following mathematical formula (Mathematical Formula 1) and the flow starting temperature Tfs of the thermoplastic resin (A) is preferably -20°C or higher, more preferably -10°C or higher, further preferably 0°C or higher, further preferably 10°C or higher, and particularly preferably 20°C or higher.
[0129] ΔT=Td5-Tfs…(Formula 1)
[0130] The difference ΔT between the 5% weight loss temperature Td5 of the silane coupling agent (C) represented by the above formula (Formula 1) and the flow start temperature Tfs of the thermoplastic resin (A) is preferably 200°C or less, more preferably 150°C or less, and further preferably 100°C or less.
[0131] By setting the difference ΔT to be -20°C or more, it is easy to prevent the adhesive layer from being colored due to a large amount of decomposition products of the silane coupling agent (C) being generated when the adhesive layer material is melt-kneaded.
[0132] By setting the difference ΔT to be 0° C. or more, the silane coupling agent (C) is less likely to volatilize when the adhesive layer material is melt-kneaded, and the amount of the silane coupling agent added to the adhesive layer can be easily controlled.
[0133] By setting the difference ΔT to be 200° C. or less, dispersibility can be easily obtained when the adhesive layer material is melt-kneaded.
[0134] The 5% weight loss temperature of the silane coupling agent (C) is preferably 120°C or higher, more preferably 140°C or higher, further preferably 150°C or higher, further preferably 160°C or higher, particularly preferably 180°C or higher.
[0135] The 5% weight loss temperature of the silane coupling agent (C) is usually 300° C. or lower.
[0136] When the 5% weight loss temperature of the silane coupling agent (C) is 120° C. or higher, stability over time is easily obtained.
[0137] When the 5% weight loss temperature of the silane coupling agent (C) is 150° C. or higher, the silane coupling agent (C) is less likely to volatilize during melt-kneading of the adhesive layer material, and the amount of the silane coupling agent added to the adhesive layer can be easily controlled.
[0138] (additive)
[0139] The high-frequency dielectric heating adhesive sheet of this embodiment may contain additives or may not contain additives. In the case where the high-frequency dielectric heating adhesive sheet of this embodiment is composed of multiple layers, at least any one of the multiple layers may contain additives or may not contain additives. In the case where at least any one of the multiple layers contains additives, the adhesive layer may contain additives or may not contain additives.
[0140] When the high-frequency dielectric heating adhesive sheet of the present embodiment includes additives, the additives include, for example, tackifiers, plasticizers, waxes, colorants, antioxidants, ultraviolet absorbers, antibacterial agents, viscosity modifiers, organic fillers, and inorganic fillers, etc. The organic fillers and inorganic fillers as additives are different from the dielectric material (dielectric filler).
[0141] Tackifiers and plasticizers can improve the melting properties and bonding properties of high-frequency dielectric heating adhesive sheets.
[0142] Examples of the tackifier include rosin derivatives, polyterpene resins, aromatic modified terpene resins, hydrogenated aromatic modified terpene resins, terpene phenol resins, coumarone-indene resins, aliphatic petroleum resins, aromatic petroleum resins, and hydrogenated aromatic petroleum resins.
[0143] As plasticizers, for example, petroleum-based process oils, natural oils, dibasic acid dialkyl esters, and low molecular weight liquid polymers can be cited. As petroleum-based process oils, for example, paraffin-based process oils, cycloparaffin-based process oils, and aromatic-based process oils can be cited. As natural oils, for example, castor oil and tall oil can be cited. As dibasic acid dialkyl esters, for example, dibutyl phthalate, dioctyl phthalate, and dibutyl adipate can be cited. As low molecular weight liquid polymers, for example, liquid polybutene and liquid polyisoprene can be cited.
[0144] In the case where the high-frequency dielectric heating adhesive sheet of the present embodiment contains additives, the content of the additives in the high-frequency dielectric heating adhesive sheet is usually preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and further preferably 0.1% by mass or more, based on the total amount of the high-frequency dielectric heating adhesive sheet. In addition, the content of the additives in the high-frequency dielectric heating adhesive sheet is preferably 20% by mass or less, more preferably 15% by mass or less, and further preferably 10% by mass or less.
[0145] The high-frequency dielectric heating adhesive sheet of this embodiment preferably does not contain a solvent. When a high-frequency dielectric heating adhesive sheet does not contain a solvent, the problem of VOC (Volatile Organic Compounds) caused by the adhesive used for bonding to the adherend is unlikely to occur.
[0146] The adhesive layer of the high-frequency dielectric heating adhesive sheet of the present embodiment preferably does not contain carbon or carbon compounds (e.g., carbon black, etc.) with carbon as the main component and conductive materials such as metals. The adhesive layer preferably does not contain, for example, carbon steel, α iron, γ iron, δ iron, copper, brass, aluminum, iron-nickel alloy, iron-nickel-chromium alloy, carbon fiber and carbon black.
[0147] When the adhesive layer contains a conductive substance, the content of the conductive substance in the adhesive layer is preferably 20 mass % or less, more preferably 10 mass % or less, further preferably 5 mass % or less, further preferably 1 mass % or less, and further preferably 0.1 mass % or less, based on the total amount of the adhesive layer.
[0148] The content of the conductive substance in the adhesive layer is particularly preferably 0 mass %.
[0149] When the content of the conductive substance in the adhesive layer is 20% by mass or less, it is easy to prevent problems such as electrical insulation breakdown during dielectric heating treatment, which may lead to carbonization of the adhesive portion and the adherend.
[0150] The total content of the thermoplastic resin (A), the dielectric filler (B) and the silane coupling agent (C) in the adhesive layer of the high-frequency dielectric heating adhesive sheet of the present embodiment is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 99% by mass or more.
[0151] As one form of the high-frequency dielectric heating adhesive sheet of this embodiment, it is composed only of a high-frequency dielectric adhesive adhesive layer. It should be noted that the high-frequency dielectric heating adhesive sheet of the present invention is not limited to a form consisting only of an adhesive layer, and other forms of the high-frequency dielectric heating adhesive sheet may also include a form in which layers other than the adhesive layer are stacked.
[0152] As described above, a high-frequency dielectric heating adhesive sheet is sometimes composed of only a high-frequency dielectric adhesive layer. Therefore, in this specification, the terms "high-frequency dielectric heating adhesive sheet" and "adhesive layer" are sometimes interchangeable.
[0153] Figure 1A to Figure 1C The schematic diagrams illustrate various forms of the high-frequency dielectric heating adhesive sheet according to the present embodiment.
[0154] Figure 1AThe high-frequency dielectric heating adhesive sheet 1A shown is composed of only a single adhesive layer 10. The high-frequency dielectric heating adhesive sheet 1A has a first surface 11 and a second surface 12 on the opposite side to the first surface 11.
[0155] The high-frequency dielectric heating adhesive sheet is preferably composed of only a single adhesive layer. By only being composed of a single adhesive layer, the thickness of the high-frequency dielectric heating adhesive sheet can be reduced and molding can be performed simply.
[0156] Figure 1B The high-frequency dielectric heating adhesive sheet 1B shown has an adhesive layer 10 and a substrate 30 supporting the adhesive layer 10. Similar to the high-frequency dielectric heating adhesive sheet 1A, the adhesive layer 10 has a first surface 11. The substrate 30 is not particularly limited as long as it is a member capable of supporting the adhesive layer 10, and examples thereof include: a resin film or resin sheet containing at least one or more resins selected from polyolefin resins such as polyethylene resins and polypropylene resins, polyester resins such as polybutylene terephthalate resins and polyethylene terephthalate resins, acetate resins, ABS resins, polystyrene resins, and vinyl chloride resins. The substrate 30 may also contain a dielectric filler (B), and the dielectric filler (B) in the adhesive layer 10 and the dielectric filler in the substrate 30 may be the same or different from each other.
[0157] Figure 1C The high-frequency dielectric heating adhesive sheet 1C shown has an adhesive layer 10, an adhesive layer 20, and an intermediate layer 40 disposed between the adhesive layer 10 and the adhesive layer 20. The high-frequency dielectric heating adhesive sheet 1C has a first surface 11 and a second surface 21 opposite to the first surface 11. The adhesive layer 10 in the high-frequency dielectric heating adhesive sheet 1C is sometimes referred to as a first adhesive layer, and the adhesive layer 20 is sometimes referred to as a second adhesive layer. In a high-frequency dielectric heating adhesive sheet having an intermediate layer arranged between a first adhesive layer and a second adhesive layer, as long as the first adhesive layer satisfies the conditions of the adhesive layer of the high-frequency dielectric heating adhesive sheet of this embodiment, in one embodiment, the first adhesive layer and the second adhesive layer are layers of the same composition and properties, in one embodiment, the second adhesive layer is a high-frequency dielectric heating adhesive layer that is different from the first adhesive layer in at least one aspect of the composition and properties, in one embodiment, the second adhesive layer is a layer of a general adhesive that is not a high-frequency dielectric heating adhesive layer, and the second adhesive layer that is not a high-frequency dielectric heating adhesive is, for example, a layer of a drying-setting adhesive that dries and solidifies upon evaporation of water or a solvent, or a layer of an adhesive formed by an adhesive (pressure-sensitive adhesive).
[0158] <Morphology and characteristics of high-frequency dielectric heating adhesive sheets>
[0159] The high-frequency dielectric heating adhesive sheet of this embodiment is composed of only one adhesive layer in one mode, and sometimes composed of multiple layers in another mode. When the high-frequency dielectric heating adhesive sheet is composed of only one adhesive layer, the adhesive layer itself is equivalent to the high-frequency dielectric heating adhesive sheet, and therefore, the form and characteristics of the high-frequency dielectric heating adhesive sheet are equivalent to the form and characteristics of the adhesive layer.
[0160] (Thickness of high frequency dielectric heating adhesive sheet)
[0161] The thickness of the high-frequency dielectric heating adhesive sheet of the present embodiment is preferably 5 μm or more, more preferably 10 μm or more, further preferably 30 μm or more, and further preferably 50 μm or more.
[0162] When the thickness of the high-frequency dielectric heating adhesive sheet is 5 μm or more, the high-frequency dielectric heating adhesive sheet can easily follow the irregularities of the adherend when bonding to the adherend, and the adhesive strength can be easily exhibited.
[0163] When the high-frequency dielectric heating adhesive sheet has a multilayer structure composed of multiple layers, the thickness of the adhesive layer is preferably 5 μm or more, more preferably 10 μm or more, further preferably 30 μm or more, and further preferably 50 μm or more.
[0164] When the high-frequency dielectric heating adhesive sheet is a multi-layered sheet, when the thickness of the adhesive layer is 5 μm or more, the adhesive layer easily follows the irregularities of the adherend during bonding to the adherend, and the adhesive strength is easily exhibited.
[0165] The upper limit of the thickness of the high-frequency dielectric heating adhesive sheet is not particularly limited. Since the thickness of the high-frequency dielectric heating adhesive sheet increases, the weight of the entire joint body obtained by bonding the high-frequency dielectric heating adhesive sheet to the adherend also increases. Therefore, the high-frequency dielectric heating adhesive sheet is preferably a thickness within a range that does not cause problems in practical use. In addition, considering the practicality and formability of the high-frequency dielectric heating adhesive sheet, the thickness of the high-frequency dielectric heating adhesive sheet is preferably 2000 μm or less, more preferably 1000 μm or less, and further preferably 600 μm or less.
[0166] (Method for manufacturing high-frequency dielectric heating adhesive sheet)
[0167] The single-layer high-frequency dielectric heating adhesive sheet can be produced by premixing the above-mentioned components, kneading them using a known kneading device such as an extruder and a heat roll, and using a known molding method such as extrusion molding, calendar molding, injection molding, and cast molding.
[0168] When the high-frequency dielectric heating adhesive sheet of the present embodiment is a multilayer structure, for example, the above-mentioned components can be premixed and manufactured by a co-extrusion method using a multilayer extruder. In addition, the single-layer sheets of each layer (for example, the first adhesive layer, the intermediate layer, and the second adhesive layer) constituting the high-frequency dielectric heating adhesive sheet of the present embodiment can be separately made, and the multiple single-layer sheets can be laminated to make them stacked, thereby manufacturing a multilayer structure sheet. When laminating the multiple single-layer sheets, for example, a heat laminator is used.
[0169] In addition, the high-frequency dielectric heating adhesive sheet of this embodiment can also be manufactured by hot extrusion coating or hot melt coating of applying a molten adhesive layer to a substrate, or by wet coating of a coating liquid obtained by dispersing or dissolving the adhesive layer composition in a solvent on a substrate.
[0170] (How to use high frequency dielectric heating adhesive sheet)
[0171] The high-frequency dielectric heating adhesive sheet of this embodiment can be used for bonding with an adherend. In addition, the high-frequency dielectric heating adhesive sheet of this embodiment can also be used for bonding a variety of adherends.
[0172] The material of the adherend is not particularly limited and may be any material of an organic material or an inorganic material (including a metal material, etc.), or may be a composite material of an organic material and an inorganic material.
[0173] As the organic material of the material of the adherend, for example, plastic materials and rubber materials can be cited. As plastic materials, for example, polypropylene resin, polyethylene resin, polyurethane resin, acrylonitrile-butadiene-styrene copolymer resin (ABS resin), polycarbonate resin (PC resin), polyamide resin (nylon 6 and nylon 66, etc.), polyester resin (polyethylene terephthalate (PET resin) and polybutylene terephthalate resin (PBT resin)), polyacetal resin (POM resin), polymethyl methacrylate resin, and polystyrene resin, etc. As rubber materials, styrene-butadiene rubber (SBR), ethylene-propylene rubber (EPR), and silicone rubber, etc. can be cited. In addition, the adherend can also be a foaming material of an organic material.
[0174] Inorganic materials as the material of the adherend include glass materials, cement materials, ceramic materials, and metal materials. In addition, the adherend can also be a fiber reinforced resin (Fiber Reinforced Plastics, FRP) as a composite material of fiber and the above-mentioned plastic material. The plastic material in the fiber reinforced resin is, for example, at least one selected from the group consisting of polypropylene resin, polyethylene resin, polyurethane resin, acrylonitrile-butadiene-styrene copolymer resin (ABS resin), polycarbonate resin (PC resin), polyamide resin (nylon 6 and nylon 66, etc.), polyester resin (polyethylene terephthalate (PET resin) and polybutylene terephthalate resin (PBT resin)), polyacetal resin (POM resin), polymethyl methacrylate resin, and polystyrene resin. The fiber in the fiber reinforced resin includes, for example, glass fiber, Kevlar fiber, and carbon fiber.
[0175] When a plurality of adherends are bonded together using the high-frequency dielectric heating adhesive sheet of the present embodiment, the plurality of adherends may be made of the same material or different materials.
[0176] The high-frequency dielectric heating adhesive sheet of this embodiment can be suitably used for bonding to glass adherends. When bonding multiple adherends, if at least one of the adherends is made of glass, the high-frequency dielectric heating adhesive sheet of this embodiment can be strongly bonded to the glass adherend.
[0177] The shape of the adherend is not particularly limited, but preferably has a surface to which the high-frequency dielectric heating adhesive sheet can be attached, and is preferably in the form of a sheet or plate. When multiple adherends are bonded to each other, the shapes and sizes of these adherends may be the same or different.
[0178] [Joining method]
[0179] The bonding method of this embodiment includes the steps of placing a high-frequency dielectric heating adhesive sheet between a first adherend and a second adherend, and applying a high-frequency electric field to the high-frequency dielectric heating adhesive sheet to bond the first adherend to the second adherend.
[0180] Hereinafter, as an example of the bonding method of this embodiment, a method of bonding the first adherend and the second adherend using a high-frequency dielectric heating adhesive sheet composed of a single adhesive layer is described, but the present invention is not limited to this method. The material of the second adherend is not particularly limited.
[0181] The bonding method according to one aspect of the present embodiment includes the following steps P1 and P2.
[0182] Process P1
[0183] Step P1 is a step of placing the high-frequency dielectric heating adhesive sheet of this embodiment between the first adherend and the second adherend. In step P1, the first adherend made of glass is brought into contact with the first surface of the high-frequency dielectric heating adhesive sheet. In addition, in step P1, the second adherend is brought into contact with the second surface of the high-frequency dielectric heating adhesive sheet.
[0184] The high-frequency dielectric heating adhesive sheet is preferably sandwiched between the first adherend and the second adherend in a manner that the first adherend and the second adherend can be bonded. The high-frequency dielectric heating adhesive sheet can be sandwiched between a portion, a plurality of portions, or the entire surface between the first adherend and the second adherend. From the viewpoint of improving the bonding strength between the first adherend and the second adherend, the high-frequency dielectric heating adhesive sheet is preferably sandwiched between the entire bonding surface of the first adherend and the second adherend.
[0185] In addition, as a method of sandwiching the high-frequency dielectric heating adhesive sheet between a portion of the first adherend and the second adherend, a method of arranging the high-frequency dielectric heating adhesive sheet in a frame shape along the periphery of the bonding surface of the first adherend and the second adherend and sandwiching the high-frequency dielectric heating adhesive sheet between the first adherend and the second adherend can be cited. By arranging the high-frequency dielectric heating adhesive sheet in a frame shape in this way, the bonding strength between the first adherend and the second adherend can be obtained, and the joint body can be made lighter than when the high-frequency dielectric heating adhesive sheet is arranged on the entire bonding surface.
[0186] In addition, by utilizing a method in which a portion of the high-frequency dielectric heating adhesive sheet is sandwiched between the first adherend and the second adherend, the size of the high-frequency dielectric heating adhesive sheet used can be reduced. Therefore, the high-frequency dielectric heating treatment time can be shortened compared to a case in which the high-frequency dielectric heating adhesive sheet is arranged on the entire bonding surface.
[0187] Process P2
[0188] Step P2 is a step of applying a high frequency electric field of 3 MHz to 300 MHz to the high frequency dielectric heating adhesive sheet interposed between the first adherend and the second adherend in step P1 to bond the first adherend and the second adherend using the high frequency dielectric heating adhesive sheet.
[0189] For example, a high-frequency electric field can be applied to the high-frequency dielectric heating adhesive sheet by using a dielectric heating bonding device. It should be noted that in this specification, a "dielectric heating device" may be referred to as a "dielectric heating bonding device" or a "high-frequency dielectric heating device".
[0190] Figure 2A schematic diagram for explaining a high-frequency dielectric heating process using the high-frequency dielectric heating adhesive sheet and the dielectric heating device according to the present embodiment is shown.
[0191] (Dielectric heating bonding device)
[0192] Figure 2 A schematic diagram of a dielectric heating bonding device 50 is shown.
[0193] The dielectric heating bonding device 50 includes a first high-frequency electric field applying electrode 51 , a second high-frequency electric field applying electrode 52 , and a high-frequency power source 53 .
[0194] The first high-frequency electric field applying electrode 51 and the second high-frequency electric field applying electrode 52 are arranged opposite to each other. The first high-frequency electric field applying electrode 51 and the second high-frequency electric field applying electrode 52 have a pressurizing mechanism. By using the pressurizing mechanism, the first adherend 110, the high-frequency dielectric heating adhesive sheet 1A and the second adherend 120 can be pressurized between the first high-frequency electric field applying electrode 51 and the second high-frequency electric field applying electrode 52.
[0195] When a pair of plate electrodes, in which the first high-frequency electric field applying electrode 51 and the second high-frequency electric field applying electrode 52 are parallel to each other, is configured, such an electrode arrangement may be referred to as a parallel plate type.
[0196] The application of the high-frequency electric field is also preferably performed using a parallel-plate type high-frequency dielectric heating device. In the case of a parallel-plate type high-frequency dielectric heating device, the high frequency penetrates the high-frequency dielectric heating adhesive sheet located between the electrodes, thereby being able to heat the entire high-frequency dielectric heating adhesive sheet, and the adherend and the high-frequency dielectric heating adhesive sheet can be bonded in a short time.
[0197] A high frequency power source 53 for applying a high frequency electric field of, for example, about 13.56 MHz, about 27.12 MHz, or about 40.68 MHz is connected to the first high frequency electric field applying electrode 51 and the second high frequency electric field applying electrode 52 .
[0198] like Figure 2 As shown, the dielectric heating bonding device 50 performs dielectric heating treatment by means of the high-frequency dielectric heating adhesive sheet 1A sandwiched between the first adherend 110 and the second adherend 120. In addition, in addition to the dielectric heating treatment, the dielectric heating bonding device 50 also bonds the first adherend 110 and the second adherend 120 by applying pressure using the first high-frequency electric field applying electrode 51 and the second high-frequency electric field applying electrode 52. It should be noted that the first adherend 110 and the second adherend 120 may be bonded together without applying pressure.
[0199] When a high-frequency electric field is applied between the first high-frequency electric field applying electrode 51 and the second high-frequency electric field applying electrode 52 , a dielectric filler (not shown) dispersed in the adhesive component of the high-frequency dielectric heating adhesive sheet 1A absorbs high-frequency energy.
[0200] The dielectric filler functions as a heat source, and the heat generated by the dielectric filler melts the thermoplastic resin component, so that the first adherend 110 and the second adherend 120 can be firmly bonded together even in a short treatment time.
[0201] Since the first high-frequency electric field applying electrode 51 and the second high-frequency electric field applying electrode 52 have a pressurizing mechanism, they also function as a pressurizing device. Therefore, by applying pressure in the compression direction by the first high-frequency electric field applying electrode 51 and the second high-frequency electric field applying electrode 52 and heating and melting the high-frequency dielectric heating adhesive sheet 1A, a stronger bonding between the first adherend 110 and the second adherend 120 can be achieved.
[0202] The joint body of the present embodiment comprises a first adherend, a second adherend, and the high-frequency dielectric heating adhesive sheet of the present embodiment. In the joint body, at least one of the first adherend and the second adherend is a glass adherend. The first adherend and the second adherend are joined together by the high-frequency dielectric heating adhesive sheet.
[0203] As one embodiment of the bonded body of the present embodiment, for example, Figure 2 The bonded body shown in the figure includes a first adherend 110, a high-frequency dielectric heating adhesive sheet 1A, and a second adherend 120.
[0204] (High frequency dielectric heating bonding conditions)
[0205] The high-frequency dielectric heating bonding conditions can be changed appropriately, but are preferably the following conditions.
[0206] The output power of the high-frequency electric field is preferably 10 W or more, more preferably 30 W or more, further preferably 50 W or more, and even more preferably 80 W or more.
[0207] The output power of the high-frequency electric field is preferably 50,000 W or less, more preferably 20,000 W or less, further preferably 15,000 W or less, further preferably 10,000 W or less, further preferably 1,000 W or less.
[0208] When the output power of the high-frequency electric field is 10 W or more, it is possible to prevent the problem that the temperature is difficult to rise during the dielectric heating treatment, so that good adhesive strength is easily obtained.
[0209] When the output power of the high-frequency electric field is 50000 W or less, it is easy to prevent the disadvantage that the temperature control becomes difficult due to the dielectric heating treatment.
[0210] The high-frequency electric field is preferably applied for a time period of 1 second or longer.
[0211] The application time of the high-frequency electric field is preferably 300 seconds or less, more preferably 240 seconds or less, further preferably 180 seconds or less, further preferably 120 seconds or less, and further preferably 100 seconds or less.
[0212] When the high-frequency electric field is applied for 1 second or longer, it is possible to prevent the problem that the temperature is difficult to rise during the dielectric heating treatment, and thus it is easy to obtain good adhesive strength.
[0213] When the application time of the high-frequency electric field is 300 seconds or less, it is easy to prevent disadvantages such as a decrease in the manufacturing efficiency of the joined body formed by bonding the first adherend and the second adherend, an increase in the manufacturing cost, and thermal degradation of the adherends.
[0214] The frequency of the high-frequency electric field to be applied is preferably 1 kHz or higher, more preferably 1 MHz or higher, further preferably 5 MHz or higher, and further preferably 10 MHz or higher.
[0215] The frequency of the applied high-frequency electric field is preferably 300 MHz or less, more preferably 100 MHz or less, further preferably 80 MHz or less, and further preferably 50 MHz or less. Specifically, the industrial frequency bands 13.56 MHz, 27.12 MHz, and 40.68 MHz allocated by the International Telecommunication Union can also be used for the high-frequency dielectric heating bonding method (bonding method) of this embodiment.
[0216] (Effects of this embodiment)
[0217] The high-frequency dielectric heating adhesive sheet of the present embodiment can be bonded to glass with high bonding strength even with low energy consumption.
[0218] Compared with the case of using an adhesive that needs to be applied, the high-frequency dielectric heating adhesive sheet of the present embodiment is easy to handle, and the workability when bonding to an adherend is also improved.
[0219] The high-frequency dielectric heating adhesive sheet of the present embodiment is superior in water resistance and moisture resistance compared to general adhesives.
[0220] The high-frequency dielectric heating adhesive sheet of this embodiment is heated by applying a high-frequency electric field, so the high-frequency dielectric heating adhesive sheet can be locally heated. Therefore, the high-frequency dielectric heating adhesive sheet of this embodiment can easily prevent the undesirable situation that the entire adherend melts when bonding with the adherend.
[0221] According to the joining method using the high-frequency dielectric heating adhesive sheet of this embodiment, it is possible to locally heat only a given portion from the outside using a dielectric heating adhesive device. Therefore, even when the adherend is a large and complex three-dimensional structure or a thick and complex three-dimensional structure, and high dimensional accuracy is required, the joining method using the high-frequency dielectric heating adhesive sheet of this embodiment is effective.
[0222] In addition, according to the high-frequency dielectric heating adhesive sheet of this embodiment, the thickness of the high-frequency dielectric heating adhesive sheet can be appropriately controlled. Therefore, the high-frequency dielectric heating adhesive sheet of this embodiment can also be applied to the roll-to-roll method, and the high-frequency dielectric heating adhesive sheet can be processed into any area and shape according to the bonding area with the adherend and the shape of the adherend by punching and the like. Therefore, from the perspective of the manufacturing process, the high-frequency dielectric heating adhesive sheet of this embodiment also has significant advantages.
[0223] [Variations of Embodiments]
[0224] The present invention is not limited to the above-described embodiments, and the present invention may include modifications and improvements within the scope that can achieve the purpose of the present invention.
[0225] The high-frequency dielectric heating adhesive sheet may have an adhesive portion. By having an adhesive portion, when the high-frequency dielectric heating adhesive sheet is sandwiched between the adherends, positional displacement can be prevented and the sheet can be configured at an accurate position. The adhesive portion may be provided on one side of the high-frequency dielectric heating adhesive sheet or on both sides. In addition, the adhesive portion may also be provided locally relative to the surface of the high-frequency dielectric heating adhesive sheet. Even in the case where the high-frequency dielectric heating adhesive sheet does not have an adhesive portion, the first adherend and the second adherend can be firmly bonded.
[0226] The high-frequency dielectric heating treatment is not limited to the dielectric heating bonding device in which the electrodes are arranged opposite to each other as described in the above embodiment, and a grid electrode type high-frequency dielectric heating device may also be used. The grid electrode type high-frequency dielectric heating device has a grid electrode, and the grid electrode is alternately arranged with electrodes of a first polarity and electrodes of a second polarity that are opposite to the first polarity at regular intervals on the same plane.
[0227] For example, when manufacturing a bonded body in which the ends of a first adherend and a second adherend are overlapped and bonded, a grid electrode type high-frequency dielectric heating device is arranged on the first adherend side or the second adherend side to apply a high-frequency electric field.
[0228] When a grid electrode type high-frequency dielectric heating device is used to bond a first adherend to a second adherend, a first grid electrode can be arranged on the first adherend side and a second grid electrode can be arranged on the second adherend side, so that the first adherend, the high-frequency dielectric heating adhesive sheet and the second adherend are sandwiched between the first grid electrode and the second grid electrode and a high-frequency electric field is applied at the same time.
[0229] When a grid electrode type high-frequency dielectric heating device is used to bond a first adherend to a second adherend, a grid electrode can be arranged on the surface side of one of the first adherend and the second adherend and a high-frequency electric field can be applied, and then a grid electrode can be arranged on the surface side of the other of the first adherend and the second adherend and a high-frequency electric field can be applied.
[0230] The high-frequency electric field is preferably applied using a grid electrode type high-frequency dielectric heating device. By using a grid electrode type high-frequency dielectric heating device, the adherends can be bonded to each other by performing dielectric heating from the surface side of the first adherend and the second adherend, for example, from the side of the adherend that is close to the high-frequency dielectric heating adhesive sheet, without being affected by the thickness of the first adherend and the second adherend. In addition, by using a grid electrode type high-frequency dielectric heating device, energy saving can be achieved in the manufacture of the joint body.
[0231] It should be noted that, for the sake of simplicity, the drawings illustrate an example of a method using a dielectric heating bonding device in which electrodes are arranged to face each other.
[0232] Example
[0233] Hereinafter, the present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples at all.
[0234] [Manufacturing of high-frequency dielectric heating adhesive sheets]
[0235] (Examples 1 to 3 and Comparative Examples 1 to 3)
[0236] The thermoplastic resin (A) and the dielectric filler (B) shown in Table 1 were premixed. The premixed material was supplied to the hopper of a 30 mm φ twin-screw extruder, and the barrel setting temperature was set to 160°C and the die temperature was set to 160°C, and the premixed material was melt-kneaded. The melt-kneaded material was cooled and then cut to produce granular pellets. Next, the produced granular pellets were put into the hopper of a single screw extruder equipped with a T-die, and a film-like molten kneaded material was extruded from the T-die while adding a silane coupling agent (C) through a liquid adding device provided in the extruder. As the temperature conditions during extrusion, the barrel temperature was set to 160°C and the die temperature was set to 160°C. The film-like molten kneaded material after extrusion was cooled using a cooling roller, thereby producing high-frequency dielectric heating adhesive sheets with a thickness of 400 μm for Examples 1 to 3 and Comparative Examples 1 to 3, respectively.
[0237] The thermoplastic resin (A), dielectric filler (B) and silane coupling agent (C) shown in Table 1 are described below.
[0238] Thermoplastic resin (A)
[0239] m-PP: Polypropylene having a maleic anhydride structure (content of monomer having maleic anhydride 10% by mass or less, MFR = 7 g / 10 min)
[0240] PP: Polypropylene without reactive sites
[0241] Dielectric filler (B)
[0242] ZnO: Zinc oxide (manufactured by Sakai Chemical Industry Co., Ltd., product name "LP-ZINC11")
[0243] Silane coupling agent (C)
[0244] SC1: 8-Glycidoxyoctyltrimethoxysilane
[0245] SC2: 3-Glycidoxypropyltrimethoxysilane
[0246] (5% weight loss temperature)
[0247] The 5% weight loss temperature Td5 was measured using a differential calorimeter (TG / DTA analyzer DTG-60 manufactured by Shimadzu Corporation).
[0248] The measurement sample was heated from 40° C. to 300° C. at a temperature increase rate of 10° C. / min at a gas flow rate of 100 ml / min in an air atmosphere, and the 5% weight loss temperature of the measurement sample was measured.
[0249] Table 2 shows the 5% weight loss temperature Td5 of the silane coupling agent (C).
[0250] (MFR: Melt Flow Rate)
[0251] The MFR of the thermoplastic resin was measured based on JIS K 7210-1:2014 using a descending flow tester (manufactured by Shimadzu Corporation, model “CFT-100D”).
[0252] (Flow start temperature)
[0253] The flow initiation temperature of the thermoplastic resin was measured using a descending flow tester (manufactured by Shimadzu Corporation, model "CFT-100D"). The load was set to 5.0 kg, a mold with a hole shape of φ2.0 mm, a length of 5.0 mm, and a barrel with an inner diameter of 11.329 mm was used, and the temperature of the measured sample was raised at a heating rate of 10°C / min, while the stroke displacement speed (mm / min) that changed with the temperature increase was measured, and a temperature dependence graph of the stroke displacement speed of the sample was obtained. The temperature at which the stroke displacement speed starts to rise again after passing through the peak obtained on the low temperature side in this graph is set as the flow initiation temperature.
[0254] The flow initiation temperature of m-PP is 153°C.
[0255] (Volume average particle size of dielectric filler)
[0256] The particle size distribution of the dielectric filler was measured by a laser diffraction / scattering method. The volume average particle size was calculated based on the results of the particle size distribution measurement in accordance with JIS Z 8819-2: 2001. The calculated volume average particle size of zinc oxide (ZnO) was 11 μm.
[0257] [Evaluation of high frequency dielectric heating adhesive sheets]
[0258] The high-frequency dielectric heating adhesive sheet was evaluated as follows. The evaluation results are shown in Table 1.
[0259] (Adhesion)
[0260] The high-frequency dielectric heating adhesive sheet was cut into a size of 25 mm × 12.5 mm and arranged between a pair of soda-lime glass (25 mm × 100 mm × 3 mm (thickness)) as adherends. After such arrangement, the pair of adherends and the high-frequency dielectric heating adhesive sheet were fixed between the electrodes of a high-frequency dielectric heating device (manufactured by Yamamoto Vinita, product name "YRP-400T-A"). The area of a pair of electrodes of the high-frequency dielectric heating device was set to 800 mm 2(=40mm×20mm), the pair of electrodes are arranged in a manner to cover the overlapping portion of the adherend (soda lime glass). With the high-frequency dielectric heating adhesive sheet and the adherend fixed between the electrodes, a high-frequency electric field is applied under the following high-frequency application conditions to bond the high-frequency dielectric heating adhesive sheet and the adherend, thereby preparing a test piece for evaluating adhesion. The pressing force when the high-frequency electric field is applied is the pressure applied to the joint of a pair of adherends.
[0261] ·High frequency electric field application conditions
[0262] Frequency: 40.68MHz
[0263] Output power: 200W
[0264] Application time: 90 seconds
[0265] Pressing pressure: 0.5MPa
[0266] The tensile shear force (unit: MPa) was measured using the test piece used for the adhesion evaluation. The tensile shear force was measured using a universal tensile testing machine (Instron company system, product name "Instron 5581"). The tensile speed in the tensile shear force measurement was set to 10 mm / min. It should be noted that the "unbonded" in the tensile shear force item in the table means that the adherend and the adhesive sheet can be easily peeled off before being used for the tensile shear force measurement.
[0267] In addition, the failure mode of the test piece for evaluating the adhesiveness in the measurement of the tensile shear force was observed, and the adhesiveness was evaluated based on the following criteria: The tensile shear force was measured based on JIS K 6850:1999.
[0268] A: The adherend is damaged.
[0269] B: The high frequency dielectric heating adhesive sheet suffered from cohesive failure.
[0270] F: The high-frequency dielectric heating adhesive sheet peels off at the interface with the adherend.
[0271] (Volatilization of materials)
[0272] In the production of the high-frequency dielectric heating adhesive sheet, the presence or absence of smoke when kneading various materials was confirmed by visual observation, and the volatilization of the materials was evaluated based on the following criteria.
[0273] A: White smoke was produced.
[0274] F: No white smoke is produced.
[0275] (Oozing)
[0276] When preparing a test piece for evaluating adhesion, the surface of the adherend around the melted high-frequency dielectric heating adhesive sheet was visually observed, and bleed-out was evaluated based on the following criteria.
[0277] A: No liquid or solid residue is generated on the surface of the adherend.
[0278] F: Liquid or solid residue is generated on the surface of the adherend.
[0279] [Table 1]
[0280]
[0281] [Table 2]
[0282]
[0283] According to the high-frequency dielectric heating adhesive sheets of Examples 1 to 3, glass adherends can be bonded to each other with high bonding strength even with low energy consumption.
Claims
1. A high-frequency dielectric heating adhesive sheet having an adhesive layer, The adhesive layer contains: A thermoplastic resin (A) having a reactive site (Y), Dielectric materials that generate heat by applying a high-frequency electric field, and Silane coupling agent (C), The reactive site (Y) comprises at least one selected from a carboxyl group, a hydroxyl group, an amino group, an isocyanate group and an acid anhydride structure, The silane coupling agent (C) comprises: Functional group (X), and Alkoxysilyl (Z), The functional group (X) is at least one group selected from epoxy, amino, isocyanate and mercapto groups, The number of atoms in the main chain linking the functional group (X) and the silicon atom of the alkoxysilyl group (Z) is 8 or more, The thermoplastic resin (A) is at least one selected from polyolefin resins, styrene resins, polyacetal resins, polycarbonate resins, polyacrylic resins, polyamide resins, polyimide resins, polyvinyl acetate resins, phenoxy resins and polyester resins.
2. The high-frequency dielectric heating adhesive sheet according to claim 1, wherein: The volume content of the silane coupling agent (C) in the adhesive layer is 0.5 volume % or more and 25 volume % or less.
3. The high-frequency dielectric heating adhesive sheet according to claim 1 or 2, wherein: The number of atoms of the main chain linking the functional group (X) and the silicon atom of the alkoxysilyl group (Z) is 15 or less.
4. The high-frequency dielectric heating adhesive sheet according to claim 1 or 2, wherein: The functional group (X) is at least one group selected from an epoxy group and an amino group.
5. The high-frequency dielectric heating adhesive sheet according to claim 1 or 2, wherein: The molecular weight of the silane coupling agent (C) is 200 or more.
6. The high-frequency dielectric heating adhesive sheet according to claim 1 or 2, wherein: The difference ΔT between the 5% weight loss temperature Td5 of the silane coupling agent (C) represented by the following mathematical formula 1 and the flow starting temperature Tfs of the thermoplastic resin (A) is -20°C or more, ΔT=Td5-Tfs…Formula 1.
7. The high-frequency dielectric heating adhesive sheet according to claim 1 or 2, wherein: The 5% weight loss temperature of the silane coupling agent (C) is above 120°C.
8. The high-frequency dielectric heating adhesive sheet according to claim 1 or 2, wherein: The reactive site (Y) includes at least one selected from a carboxyl group and an acid anhydride structure.
9. The high-frequency dielectric heating adhesive sheet according to claim 1 or 2, wherein: The reactive site (Y) comprises a maleic anhydride structure.
10. The high-frequency dielectric heating adhesive sheet according to claim 1 or 2, wherein: The thermoplastic resin (A) is a polyolefin resin.
11. The high-frequency dielectric heating adhesive sheet according to claim 1 or 2, wherein: The volume content of the dielectric material in the adhesive layer is 5 volume % or more and 50 volume % or less.
12. The high-frequency dielectric heating adhesive sheet according to claim 1 or 2, wherein: The dielectric material is a dielectric filler (B).
13. The high-frequency dielectric heating adhesive sheet according to claim 12, wherein: The dielectric filler (B) includes at least one selected from zinc oxide, silicon carbide, barium titanate, and titanium oxide.
14. The high-frequency dielectric heating adhesive sheet according to claim 12, wherein: The volume average particle size of the dielectric filler (B) is 1 μm or more and 30 μm or less, The volume average particle size is a volume average particle size calculated based on the particle size distribution measurement results of the dielectric filler (B) by a laser diffraction / scattering method and in accordance with JIS Z 8819-2:2001.
15. A method of joining, comprising: A step of disposing the high-frequency dielectric heating adhesive sheet according to any one of claims 1 to 14 between a first adherend and a second adherend; and A step of applying a high-frequency electric field to the high-frequency dielectric heating adhesive sheet to bond the first adherend to the second adherend.
16. A conjugate comprising: The first adherend, a second adherend, and The high-frequency dielectric heating adhesive sheet according to any one of claims 1 to 14, in, At least one of the first adherend and the second adherend is a glass adherend, The first adherend and the second adherend are bonded together by the high-frequency dielectric heating adhesive sheet.