A method for preparing soybean oil-based alkyd resin polyester by a step-by-step method

Soybean oil-based alkyd resin bulk polyester is prepared in a solvent-free system by step-by-step method, using alcohol-anhydride prepolymerization and epoxy soybean oil ring-opening polymerization, the problems of insufficient rigidity and dependence on fossil resources were solved, and the problem of traditional polyurethane materials was achieved. High performance and degradable biomass-based materials.

CN115819737BActive Publication Date: 2024-11-08FUZHOU UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211377151.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-04
Publication Date
2024-11-08
Estimated Expiration
2042-11-04

AI Technical Summary

Technical Problem

Traditional polyurethane materials have strong dependence on fossil resources and have poor degradation performance. The lack of aromatic ring structure leads to insufficient rigidity, which limits its practical application.

Method used

Soybean oil-based alkyd resin body polyester is prepared in a solvent-free system by step-by-step method, forming oligomers through alcohol-anhydride prepolymerization, and ring-opening polymerization with epoxy soybean oil, introducing aromatic ring structures, and improving the mechanics of the material performance.

Benefits of technology

The preparation of soybean oil-based alkyd resin body polyester with good mechanical properties under solvent-free conditions is achieved, which reduces the sublimation problem of acid anhydride, reduces the dependence of fossil resources, and improves the rigidity and degradability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 221104075333
    Figure 221104075333
  • Figure 221104075337
    Figure 221104075337
  • Figure 221104075340
    Figure 221104075340
Patent Text Reader

Abstract

The present invention discloses a method for preparing soybean oil-based alkyd resin polyester by a step-by-step method, wherein polyol, anhydride and accelerator are mixed and ground uniformly, and then reacted to obtain a primary reaction product, and then the obtained primary reaction product is preheated and cured with epoxidized soybean oil to obtain the soybean oil-based alkyd resin polyester. The present invention uses renewable biomass-based raw materials to prepare polyester materials, which conforms to the concept of green and sustainable development; and the solvent-free method is used to prepare alkyd resin in the preparation process, which effectively solves the sublimation problem of anhydride during heating and reduces environmental pollution; alcohol and anhydride are used to form oligomers, and the branching degree and functionality are adjustable; the prepared polyester material has a three-dimensional cross-linked network structure and has good mechanical properties and water resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of biomass-based polyester material preparation, and specifically relates to a method for preparing alkyd resin-type polyester in steps by utilizing alcohol-anhydride-epoxy vegetable oil. Background Art

[0002] Polymer materials are widely used in many fields such as communications, electronics, aviation, medical treatment, and chemical industry. Among them, as a commonly used polymer material, polyester plays an important role in human economic and social development. Traditional polyurethane materials are highly dependent on fossil resources and have poor degradation performance. After being discarded, they will pollute the environment and are not conducive to human health. Therefore, reducing the dependence of traditional polymer materials on fossil resources and developing and utilizing renewable biomass is an important direction for the future. It is of great significance to achieve "carbon peak" and "carbon neutrality" and is in line with the current mainstream of green and sustainable development. Introducing biomass into the preparation of polymer materials such as polylactic acid, polyglycolic acid, and polybutylene glycol succinate not only reduces production costs, but also improves the degradability of materials, thereby reducing the use of fossil resources and is conducive to protecting the environment. However, due to the lack of aromatic ring structure in these materials, they lack rigidity, which limits their practical application. Therefore, it is of great significance to develop new biomass-based polymer materials with low price and good degradation performance.

[0003] Epoxy resins are usually polycondensed with epichlorohydrin and bisphenol A or polyols. However, compounds containing active hydrogen generally have the potential to undergo ring-opening polymerization with epoxy groups and can be cured to form a three-dimensional cross-linked structure. Therefore, new polymer materials can be synthesized by adjusting compounds containing epoxy functional groups or active hydrogen. Vegetable oil is an important renewable resource with a wide range of applications. The main component of vegetable oil is the ester formed by straight-chain fatty acids and glycerol, and its molecular chain contains functional groups such as ester groups and double bonds. Due to different plant species, the length of fatty acid chains and the number of double bonds in different vegetable oils vary. After epoxidation of vegetable oil, epoxy vegetable oil containing epoxy groups can usually be obtained. Different polymer materials can be obtained by further anionic or cationic ring-opening polymerization of epoxy groups with alcohols, carboxylic acids, etc.

[0004] Epoxidized soybean oil is a widely used biomass-based raw material in the industrial field. It has no aromatic ring in its molecular chain and has a small molecular weight. The types of curing agents commonly used for general epoxy resins include amine curing agents, acid anhydride curing agents, synthetic resin curing agents, etc. In order to prepare soybean oil-based polyester materials with good rigidity, anhydrides containing benzene rings can be used as curing agents. However, solid acid anhydrides such as phthalic anhydride are easy to sublimate during heating and cannot fully undergo polymerization reactions in solvent-free polymerization systems. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing soybean oil-based alkyd resin bulk polyester, which adopts a step-by-step method to prepare soybean oil-based alkyd resin bulk polyester with good mechanical properties in a solvent-free system.

[0006] To achieve the above object, the present invention adopts the following technical solution:

[0007] A soybean oil-based alkyd resin-based polyester prepared by a step-by-step method, the preparation method comprising the following steps:

[0008] (1) After the polyol, acid anhydride and accelerator are mixed and ground evenly, the mixture is reacted at 80-140°C for 20-60 minutes to obtain an initial reaction product;

[0009] (2) The initial reaction product obtained in step (1) is preheated to 50-80° C., mixed with epoxidized soybean oil, and then cured to obtain the soybean oil-based alkyd resin polyester.

[0010] Furthermore, in parts by weight, the usage of each raw material is 8.24 to 42.44 parts of polyol, 29.60 to 64.28 parts of acid anhydride, 0.17 to 2.04 parts of accelerator, and 61.20 to 163.00 parts of epoxidized soybean oil.

[0011] Furthermore, the polyol is one or more liquid polyols such as ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, diethylene glycol, glycerol, etc.

[0012] Furthermore, the acid anhydride is phthalic anhydride.

[0013] Furthermore, the promoter is one or more of zinc acetate, iron acetate, cobalt acetate, nickel acetate and the like.

[0014] Furthermore, the epoxy value of the epoxidized soybean oil is ≥6.0% and the acid value is ≤5.0 mg KOH / g.

[0015] Furthermore, the curing may be performed at room temperature for 5 to 14 days; or first at 80 to 100° C. for 3 to 5 hours, then at 100 to 130° C. for 2 to 3 hours, and then at 130 to 180° C. for 1 to 2 hours; or at 120 to 140° C. for 3 to 5 hours.

[0016] When polyols and anhydrides react, the 2-2 functionality system can only form linear polymers in principle; the 2-3 or 2-4 functionality system can form not only linear polymers but also stereopolymers. The present invention first reacts the anhydride with the alcohol to polymerize to produce a multifunctional carboxyl-terminated oligomer with a branched structure. The oligomer is not easy to sublime under heating and has a large number of aromatic rings and carboxyl groups in the molecular structure; then the oligomer is ring-opened polymerized with epoxy soybean oil to form a polyester with a three-dimensional cross-linked network structure. At this time, the epoxy soybean oil acts as a cross-linking agent, and the introduction of the aromatic ring structure in its molecular chain improves the rigidity of the material and enhances the mechanical properties of the material. It effectively solves the sublimation problem of solid anhydrides, so that soybean oil-based alkyd resin can be prepared without an organic solvent. The addition of the accelerator reduces the reaction activation energy, accelerates the reaction rate, reduces the reaction temperature, and reduces the reaction energy consumption.

[0017] Compared with directly using phthalic anhydride to cure epoxidized soybean oil, the method of using epoxidized soybean oil to cure oligomers of polyols and anhydrides to prepare soybean oil-based alkyd resin effectively reduces the sublimation of anhydrides, and its branching degree and functionality are variable and flexibly regulated.

[0018] Aiming at the deficiency of the materials in the background, the present invention has the following advantages:

[0019] (1) The present invention uses renewable epoxidized soybean oil, which reduces dependence on fossil resources and conforms to the concept of green and sustainable development.

[0020] (2) The present invention adopts a two-step reaction and utilizes alcohol-acid anhydride prepolymerization to form oligomers, which effectively reduces the sublimation problem of acid anhydride during the heating process, thereby enabling the preparation of soybean oil-based alkyd resin by a solvent-free method.

[0021] (3) The reaction temperature required by the present invention is lower and the energy consumption is less.

[0022] (4) The present invention introduces an aromatic ring structure into the polyester molecular chain, thereby enhancing the rigidity of the polyester material. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a sample picture of the soybean oil-based alkyd resin obtained in Example 1.

[0024] Figure 2 This is a sample picture of the soybean oil-based alkyd resin obtained in Example 2.

[0025] Figure 3 This is a sample picture of the soybean oil-based alkyd resin obtained in Example 3.

[0026] Figure 4 This is a sample picture of the soybean oil-based alkyd resin obtained in Example 4.

[0027] Figure 5 This is a sample picture of the soybean oil-based alkyd resin obtained in Example 5.

[0028] Figure 6 This is a comparison of the sublimation of anhydride in the comparative example. DETAILED DESCRIPTION

[0029] A method for preparing soybean oil-based alkyd resin by a step-by-step method comprises the following steps:

[0030] (1) 8.24-42.44 parts by weight of polyol, 29.60-64.28 parts by weight of acid anhydride, and 0.17-2.04 parts by weight of accelerator are mixed and ground evenly, and stirred at 80-140° C. for 20-60 min to obtain an initial reaction product, which is then cooled to room temperature; the stirring reaction speed is 150-600 rpm;

[0031] (2) The initial reaction product obtained in step (1) is preheated to 50-80° C., and then mixed with 61.20-163.00 parts by weight of epoxy soybean oil and then cured to obtain the soybean oil-based alkyd resin.

[0032] The polyol is one or more liquid polyols such as ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, diethylene glycol, glycerol, etc.

[0033] The acid anhydride is phthalic anhydride.

[0034] The promoter is one or more of zinc acetate, iron acetate, cobalt acetate, nickel acetate and the like.

[0035] The epoxy value of the epoxidized soybean oil is ≥6.0% and the acid value is ≤5.0 mg KOH / g, and the epoxidized soybean oil needs to be vacuum dehydrated before use.

[0036] The curing may be performed at room temperature for 5 to 14 days; or first at 80 to 100° C. for 3 to 5 hours, then at 100 to 130° C. for 2 to 3 hours, and then at 130 to 180° C. for 1 to 2 hours; or at 120 to 140° C. for 3 to 5 hours.

[0037] In order to make the contents of the present invention easier to understand, the technical solution of the present invention is further described below in conjunction with specific implementation methods, but the present invention is not limited thereto.

[0038] Example 1

[0039] (1) Take 18.4 parts of glycerol, 59.2 parts of phthalic anhydride, and 0.34 parts of zinc acetate, add them into a reactor equipped with a stirring device, set the stirring speed to 200 rpm, set the heating temperature to 120°C, react for 20 minutes, and then cool to room temperature to obtain an initial reaction product.

[0040] (2) The initial reaction product obtained in step (1) was preheated to 60° C., 162.9 parts of epoxidized soybean oil was added, the stirring speed was set to 400 rpm, and after mixing evenly, the mixture was cured at 120° C. for 3 h to obtain a soybean oil-based alkyd resin.

[0041] Example 2

[0042] (1) Take 18.4 parts of glycerol, 59.2 parts of phthalic anhydride, and 0.34 parts of zinc acetate, add them into a reactor equipped with a stirring device, set the stirring speed to 200 rpm, set the heating temperature to 120°C, react for 25 minutes, and then cool to room temperature to obtain an initial reaction product.

[0043] (2) The initial reaction product obtained in step (1) was preheated to 60°C, 122.2 parts of epoxidized soybean oil was added, the stirring speed was set to 400 rpm, and after mixing evenly, the mixture was cured at 120°C for 3 h to obtain a soybean oil-based alkyd resin.

[0044] Example 3

[0045] (1) Take 18.4 parts of glycerol, 59.2 parts of phthalic anhydride, and 0.34 parts of zinc acetate, add them into a reactor equipped with a stirring device, set the stirring speed to 200 rpm, set the heating temperature to 120°C, and react for 25 minutes to obtain an initial reaction product.

[0046] (2) The initial reaction product obtained in step (1) was preheated to 60° C., 142.6 parts of epoxidized soybean oil was added, the stirring speed was set to 400 rpm, and after mixing evenly, the mixture was cured at 120° C. for 3 h to obtain a soybean oil-based alkyd resin.

[0047] Example 4

[0048] (1) Take 18.4 parts of glycerol, 59.2 parts of phthalic anhydride, and 0.34 parts of zinc acetate, add them into a reactor equipped with a stirring device, set the stirring speed to 200 rpm, set the heating temperature to 120°C, react for 25 minutes, and then cool to room temperature to obtain an initial reaction product.

[0049] (2) The initial reaction product obtained in step (1) was preheated to 60°C, 122.2 parts of epoxidized soybean oil was added, the stirring speed was set to 400 rpm, and after mixing evenly, it was first cured at 120°C for 2 h and then cured at 140°C for 1 h to obtain a soybean oil-based alkyd resin.

[0050] Example 5

[0051] (1) Take 18.4 parts of glycerol, 59.2 parts of phthalic anhydride, and 0.34 parts of zinc acetate, add them into a reactor equipped with a stirring device, set the stirring speed to 200 rpm, set the heating temperature to 120°C, react for 25 minutes, and then cool to room temperature to obtain an initial reaction product.

[0052] (2) The initial reaction product obtained in step (1) was preheated to 60°C, 122.2 parts of epoxidized soybean oil was added, the stirring speed was set to 400 rpm, and after mixing evenly, it was first cured at 120°C for 3 h, then cured at 120°C for 2 h, and finally cured at 140°C for 1 h to obtain a soybean oil-based alkyd resin.

[0053] The standard tensile specimens were prepared according to the method described in the example, and then the mechanical properties were tested at a test speed of 5 mm / min according to GB / T1040.3-2006. The results are shown in Table 1.

[0054] Table 1 Mechanical properties test results of soybean oil-based alkyd resin obtained in Example

[0055]

[0056] The specimens obtained in the example were immersed in water, taken out at intervals, weighed, and their swelling properties were tested and the swelling ratio was calculated according to the following formula. The results are shown in Table 2.

[0057]

[0058] Table 2 Test results of swelling properties of soybean oil-based alkyd resin obtained in Example in water

[0059]

[0060] It can be seen from Tables 1 and 2 that the epoxy soybean oil-based alkyd resin provided by the present invention has good mechanical strength and water resistance.

[0061] Comparative Example

[0062] (1) Take 18.4 parts of glycerol, 59.2 parts of phthalic anhydride, and 0.34 parts of zinc acetate, add them into a reactor equipped with a stirring device, set the stirring speed to 200 rpm, set the heating temperature to 120°C, react for 20 min, and then cool to room temperature.

[0063] (2) Heat 59.2 parts of phthalic anhydride at 120°C for 20 min, and compare the sublimation conditions in (1) and (2).

[0064] Depend on Figure 6It can be seen that phthalic anhydride is easy to sublimate when heated, and a large amount of needle-shaped phthalic anhydride solids are formed when the tube wall is cooled, while the pre-reaction product of glycerol and phthalic anhydride does not have obvious phthalic anhydride sublimation after heating. This method effectively reduces the sublimation of phthalic anhydride and reduces environmental pollution.

[0065] The present invention adopts a two-step reaction to effectively reduce the sublimation problem of anhydride, thereby reducing harm to human body and environment; adopts renewable biomass-based materials to reduce dependence on fossil resources, which is in line with the concept of green development; the introduction of a large number of aromatic rings increases the rigidity of the material and expands the application range of the material; alcohol-anhydride forms oligomers, and the branching degree and functionality are flexibly adjustable. Therefore, the present invention has many advantages such as easy availability of raw materials, simple preparation method, low reaction temperature, etc.

[0066] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.

Claims

1. A method for preparing soybean oil-based alkyd resin polyester by a step-by-step method, characterized in that: The following steps are involved: (1) After the polyol, acid anhydride and accelerator are mixed and ground evenly, the mixture is reacted at 80-140°C for 20-60 minutes to obtain an initial reaction product; (2) preheating the initial reaction product obtained in step (1) to 50-80° C., stirring and mixing the product with epoxidized soybean oil, and then curing the mixture to obtain the soybean oil-based alkyd resin polyester; By weight, the amount of each raw material is 8.24-42.44 parts of polyol, 29.60-64.28 parts of acid anhydride, 0.17-2.04 parts of accelerator, and 61.20-163.00 parts of epoxidized soybean oil; The polyol is glycerol; the acid anhydride is phthalic anhydride; and the accelerator is one or more of zinc acetate, ferric acetate, cobalt acetate and nickel acetate.

2. The method for preparing soybean oil-based alkyd resin-based polyester by a stepwise method according to claim 1, characterized in that: The epoxy value of the epoxidized soybean oil is ≥6.0% and the acid value is ≤5mg KOH / g.

3. A soybean oil-based alkyd resin-based polyester prepared by the method as claimed in claim 1.