A method for improving the purity and uniformity of mirror die steel

Through multiple smelting in non-vacuum induction furnace, LF furnace, VD furnace and protective atmosphere electroslag furnace combined with high-temperature homogenization, forging and ultra-fine refinement processes, the problem of insufficient purity and structural uniformity of mirror mold steel has been solved, significantly. Improve the quality and economic benefits of mold steel.

CN115821147BActive Publication Date: 2024-10-18SICHUAN JIANGYOU LIUHE STEAM TURBINE MATERIAL
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211557499.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-06
Publication Date
2024-10-18
Estimated Expiration
2042-12-06

AI Technical Summary

Technical Problem

The existing mirror mold steel has low purity and poor structural uniformity, and cannot meet the high-quality requirements of high-end mold steel, resulting in insufficient polishing performance and service life, and high production costs.

Method used

A non-vacuum induction furnace + LF furnace + VD furnace is used for primary smelting, followed by secondary remelting in a protective atmosphere electroslag furnace, and then third remelting in a vacuum consumable furnace, combining high-temperature homogenization, cooling forging and ultra-fine chemical process to prepare mirror mold steel with high purity and structural uniformity.

Benefits of technology

The purity and structural uniformity of mold steel are significantly improved. The inclusion level reaches Class A, the structural level reaches SA1 level, and the grain size reaches level 10. It reduces production costs and improves economic and social benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GHA0000006321080000061
    Figure GHA0000006321080000061
  • Figure GHA0000006321080000071
    Figure GHA0000006321080000071
  • Figure GHA0000006321080000141
    Figure GHA0000006321080000141
Patent Text Reader

Abstract

The invention discloses a method for improving the purity and organization of mirror die steel, which is to first use a non-vacuum induction furnace + LF furnace + VD furnace for smelting, then use a protective atmosphere electric slag furnace for secondary remelting, and then use a vacuum consumable furnace for tertiary remelting to obtain a uniform and very high purity steel ingot, and finally obtain a 4T large module with very high organization uniformity and purity through high temperature homogenization, temperature reduction forging, water cooling after forging and ultra-fine processing. The steel has extremely high purity and good organization uniformity. The organization level can reach SA1 level by sampling and testing according to the SEP1614 hot working die steel microscopic detection and evaluation standard rating chart microscopic inspection method, the mesh level can reach 1 level by sampling and testing according to the GB / T1299 alloy tool steel standard rating chart microscopic inspection method, and the grain size level can reach 10 level by rating according to the GB / T6394-2002 metal average grain size determination method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of mold steel materials, and relates to a production process of mirror mold steel, and specifically to a method for improving the purity and structural uniformity of mirror mold steel (4Cr13 series large modules), such as mirror mold steel for car lights. Background Art

[0002] With the rapid development of my country's plastics industry and the gradual maturity of professional mold manufacturing technology, the industrial demand for plastic product molding is increasing, and the quality requirements for plastic mold steel are also getting higher and higher.

[0003] Traditional plastic mold steel is increasingly unable to meet the high quality requirements of complex structure, high dimensional accuracy, high corrosion resistance, high polishing rate, etc. Especially for high-end mirror plastic mold steel, the current production capacity is limited, the product quality is uneven, and the polishing performance and service life still need to be further improved; at the same time, the polishing cost accounts for 5-30% of the mold cost, resulting in the high production cost of this type of steel. Therefore, it is imperative to develop new technologies, new processes, and new varieties of high-end mold steel such as high mirror.

[0004] The service life of mirror mold steel is closely related to its surface quality. In the production process of mirror mold steel, the failure of the mold is mainly related to its polishing performance, and the failure forms mainly include scar defects, pitting, holes, orange peel, etc. Relevant research shows that in the polishing process of mirror plastic mold steel, the scar convex defects on the mold surface are closely related to TiN inclusions and their composite inclusions, CaO-SiO2-Al2O local segregation three types of inclusions inside the steel, and the rich and uneven composition of harmful elements such as P and S. These factors lead to early failures on the mold surface. The presence of pitting and holes leads to a decrease in the polishing quality and corrosion resistance of the mold surface, which is due to large silicate inclusions, residual oxides and severe local decarburization.

[0005] However, although the existing production process has been greatly improved, it still cannot solve the defects of low purity and easily affected structural uniformity of mirror mold steel. Therefore, how to improve the purity and structural uniformity of mirror mold steel has become a technical problem that needs to be solved urgently. Summary of the invention

[0006] The purpose of the present invention is to solve the above-mentioned technical problems, thereby providing a method for improving the purity and structural uniformity of mirror mold steel to meet the use requirements in the field of high-end mold steel products.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A method for improving the purity and uniformity of mirror mold steel, wherein the element composition of the mirror mold steel includes, by weight percentage: C: 0.35-0.40%, Mn: 0.30-0.80%, Si: 0.70-1.00%, S: ≤0.003%, P: ≤0.025%, Cr: 13.00-14.00%, Ni: ≤0.50%, Mo: ≤0.50%, V: 0.25-0.35%, Cu: ≤0.20%, Al: ≤0.03%, and the balance is iron and unavoidable residual elements;

[0009] The method for improving the purity and structural uniformity of mirror mold steel comprises the following steps:

[0010] (1) preparing an alloy according to the above elemental composition, melting it in a non-vacuum induction furnace at a melting temperature of 1510-1520° C., adding slag during the melting process for deoxidation and desulfurization, removing ≥90% of the slag after the material is cleared, then adding slag again to make slag, adding Al powder for diffusion deoxidation, heating to 1560-1580° C. for sampling and analysis, further heating to above 1620° C., tapping the steel into an LF furnace;

[0011] (2) After the ladle is placed in the LF station, the temperature is raised to adjust the slag, and the composition is adjusted according to the sampling results. Carbon powder, Al powder, and Si-Ca powder are added for diffusion deoxidation to maintain a reducing atmosphere. The slag is sampled, the temperature is raised to 1670-1690℃, and the slag is removed by ≥60%. The steel is then discharged and sent to the VD station;

[0012] (3) Before the VD furnace is evacuated, 0.5 kg / t of rare earth is placed in the bag. The total evacuation time is ≥30 min, the ultimate vacuum is ≤133 Pa, and the holding time is ≥10 min. After the vacuum is broken, the temperature is measured, and argon gas is blown for ≥10 min. The temperature is measured at 1525-1530 ° C, and the steel is poured;

[0013] (4) The electrode rod is demoulded 4 hours after casting, slowly cooled to 200-300°C and then put into a furnace for annealing. After annealing, the ends of the electrode rod are flattened and the surface is polished;

[0014] (5) placing the electrode rod as an electrode in a protective atmosphere electroslag remelting furnace for secondary remelting and purification to form an electroslag ingot;

[0015] (6) The electroslag ingot is loaded into the furnace for annealing within 24 hours after the cover is removed. After annealing, the two ends of the electroslag ingot are flattened and the surface is polished;

[0016] (7) placing the electroslag ingot as an electrode in a vacuum consumable remelting furnace for remelting, purification, and degassing to form a consumable ingot;

[0017] (8) The consumable ingot is taken out of the hood and air-cooled to 150-250°C before being put into the furnace for annealing. After annealing, the surface is polished;

[0018] (9) The treated steel ingot is placed in a heating furnace, heated to 500°C at ≤80°C / h and kept at this temperature for 4 hours, then heated to 850°C at ≤100°C / h and kept at this temperature for 6 hours, and finally heated to 1280°C at ≤150°C / h and kept at this temperature for 35 hours, then the furnace door is opened and the temperature is lowered to 1180°C and kept at this temperature for 1 hour before being taken out of the furnace for forging;

[0019] (10) After forging, water cooling is carried out. After the forging is completed, the module is first returned to 550°C, and then air-cooled until the surface temperature reaches 250-350°C and then annealed in a furnace. After annealing, flaw detection, flattening, and grinding are carried out;

[0020] (11) The module processed in step (10) is subjected to ultra-fine processing to prepare a mirror mold steel with high purity and good structural uniformity.

[0021] The method provided by the present invention first adopts a non-vacuum induction furnace + LF furnace + VD furnace for smelting, then adopts a protective atmosphere electric slag furnace for secondary remelting, and then adopts a vacuum consumable furnace for tertiary remelting to obtain a uniform and very high purity steel ingot, and finally obtains a 4T large module with very high uniformity and purity through high-temperature homogenization, temperature reduction forging, water cooling after forging and ultra-fine processing. The inclusion level is sampled and inspected according to the ASTM E45 steel non-metallic inclusion content determination standard rating chart microscopic inspection method. It is found that the steel has extremely high purity and good structural uniformity. The structural level is sampled and inspected according to the SEP1614 hot working die steel microscopic detection and evaluation standard rating chart microscopic inspection method, and can reach SA1 level. The mesh level is sampled and inspected according to the GB / T1299 alloy tool steel standard rating chart microscopic inspection method, and can reach level 1. The grain size level is rated according to the GB / T 6394-2002 metal average grain size determination method and can reach level 10.

[0022] Furthermore, the residual elements include: Ti: ≤0.008%, Nb: ≤0.01%, H: ≤0.0001%, O: ≤0.0015%, N: ≤0.01%.

[0023] Furthermore, in step (1), the molten steel is melted in a 20 t non-vacuum induction furnace, and pre-slag is made using a 3 t furnace mixed blast furnace.

[0024] Furthermore, in step (2), the white slag retention time during the LF furnace refining period is ≥30 min.

[0025] Furthermore, in step (4), the annealing temperature is 700-750°C, the holding time is ≥20h, and the furnace is cooled to 500°C at a rate of ≤30°C / h and then air-cooled out of the furnace.

[0026] Furthermore, in step (5), the protective atmosphere electroslag remelting uses 66 #Pre-melted slag, melting rate is 7.0 ~ 6.5kg / min, electroslag is finished, furnace cooling ≥ 90min and then hood cooling, hood cooling time ≥ 72h.

[0027] Furthermore, in step (6) and step (8), the annealing temperature is 700-750°C, the holding time is ≥24h, and the furnace is cooled to 500°C at a rate of ≤30°C / h and then air-cooled.

[0028] Furthermore, in step (7), the maximum arc starting current during the vacuum consumable remelting process is 15000±1000A, and the melting rate is 7.0-6.7kg / min.

[0029] Furthermore, in step (9), the forging process is a two-fire forming process of one punch and one pull, and the start forging temperature is ≥1050°C, and the final forging temperature is 800-850°C; in step (11), the ultra-fine process is a quenching and a tempering process.

[0030] Furthermore, in step (10), the water cooling time is calculated based on the module thickness of 4min / 100mm, and air cooling is performed for 3min before water cooling; the annealing temperature is 700-750°C, the holding time is ≥24h, and the furnace is cooled to 500°C at ≤30°C / h and then air-cooled out of the furnace.

[0031] The beneficial effects of the present invention are as follows:

[0032] (1) The mold steel material prepared by the method provided by the present invention has extremely high purity. The inclusion level of the mold steel material produced by the method of the present invention can reach the following level by sampling and inspection according to the ASTM E45 standard rating chart microscopic inspection method for determining the content of non-metallic inclusions in steel: non-metallic inclusions of types A, B, C and DS are all 0, the coarse particles of type D are 0, and the fine particles are 0.5;

[0033] (2) The mold steel obtained by the method of the present invention has good uniformity of organization. Its organization level can reach SA1 level by sampling and testing according to the microscopic inspection method of the SEP1614 hot working die steel microscopic inspection and evaluation standard rating chart; its mesh level can reach 1 level by sampling and testing according to the microscopic inspection method of the GB / T1299 alloy tool steel standard rating chart; its grain size level can reach 10 level by rating according to the GB / T 6394-2002 metal average grain size determination method;

[0034] (3) The mold steel material produced by the method of the present invention has good economic and social benefits in the high-end mirror mold steel market and is suitable for promotion and use. DETAILED DESCRIPTION

[0035] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] The alloy raw materials of mold steel are prepared according to the weight percentage of each element composition in Table 1 below:

[0037] Table 1

[0038]

[0039]

[0040] Example 1

[0041] The steps for preparing sample 1 are as follows:

[0042] Step A, preparing the alloy according to the above-mentioned element composition ratio, melting and homogenizing in a non-vacuum induction furnace, the melting temperature is 1510°C, and slag needs to be continuously added during the melting process for deoxidation and desulfurization, and 90% of the slag is removed after the material is cleared, and slag is added again to make slag, and an appropriate amount of Al powder is added for diffusion deoxidation, fully stirred, heated to 1560°C, sampled and analyzed, and then heated to 1620°C, and the steel is tapped into the LF furnace;

[0043] Step B, after the ladle is placed in the LF station, the temperature is increased and the slag is adjusted. The composition is adjusted according to the sampling results of step A, and carbon powder, Al powder, and Si-Ca powder are added for diffusion deoxidation to maintain a reducing atmosphere. The slag white is sampled, and the temperature is increased to 1670°C to remove 60% of the slag and tap the steel into the VD station;

[0044] Step C, evacuate the VD furnace before placing 0.5kg / T of rare earth in the bag, the total evacuation time is 30min, the ultimate vacuum is 133Pa, the holding time is 10min, the temperature is measured after breaking the vacuum, argon is blown for 10min, and the temperature is measured at 1525℃ for steel pouring;

[0045] Step D: After pouring for 4 hours, the electrode rod is demoulded, slowly cooled to 200°C and immediately put into a furnace for annealing. After annealing, the ends of the electrode rod are flattened and the surface is polished;

[0046] Step E, placing the electrode rod processed in step D as an electrode in a protective atmosphere electroslag remelting furnace for secondary remelting and purification to form an electroslag ingot;

[0047] Step F, after the electroslag ingot is removed from the cover, it is loaded into the furnace for annealing within 24 hours, and after annealing, both ends of the electroslag ingot are flattened and the surface is polished;

[0048] Step G, placing the electroslag ingot treated in step F as an electrode in a vacuum consumable remelting furnace for remelting, purification, and degassing to form a consumable ingot;

[0049] Step H, the consumable ingot is taken out of the hood and air-cooled to 150°C, and then immediately put into the furnace for annealing. After the annealing is completed, the surface is polished and the next production process is transferred;

[0050] Step I: Place the steel ingot processed in step H in a heating furnace, heat it to 500°C at 80°C / h and keep it for 4 hours, then heat it to 850°C at 100°C / h and keep it for 6 hours, finally heat it to 1280°C at 150°C / h and keep it for 35 hours, then open the furnace door and cool it to 1180°C and keep it for 1 hour before taking it out of the furnace for forging;

[0051] Step J: After forging is completed, the mold is put into water for treatment. After water cooling, the mold is first returned to 550°C, then air-cooled to a surface temperature of 250°C and immediately put into a furnace for annealing. After annealing, flaw detection, flattening, and grinding are performed;

[0052] Step K: subjecting the module processed in step J to ultrafine processing to obtain the required material.

[0053] Among them, in step A, the molten steel is melted in a 20T non-vacuum induction furnace, and pre-slag is made by using a 3T furnace mixed blasting.

[0054] Wherein, in step B, the white slag is maintained for 30 minutes during the LF furnace refining period.

[0055] Among them, in step C, hydrogen needs to be measured after the VD furnace is broken.

[0056] Wherein, in step D, the annealing temperature is 700° C., the holding time is 20 h, and the furnace is cooled to 500° C. at 30° C. / h and then air-cooled out of the furnace.

[0057] Among them, in step E, the protective atmosphere electroslag remelting uses 66 # Pre-melting slag, melting rate is 7.0kg / min, electroslag is finished, furnace cooling is 90min and then hood cooling, hood cooling time is 72h.

[0058] In step F, the annealing temperature is 700° C., the holding time is 24 h, and the furnace is cooled to 500° C. at 30° C. / h and then air-cooled out of the furnace.

[0059] Among them, in step G, the maximum allowable arc current during the vacuum consumable remelting process is 15000±1000A, and the melting rate is 7.0kg / min.

[0060] In step H, the annealing temperature is 700° C., the holding time is 24 h, and the furnace is cooled to 500° C. at 30° C. / h and then air-cooled out of the furnace.

[0061] Among them, in step I, the forging process is one-piercing and one-pulling two-fire forming, and the starting forging temperature is 1050°C and the final forging temperature is 800°C.

[0062] Among them, in step J, the water cooling time is calculated based on the module thickness of 4min / 100mm, and air cooling is performed for 3min before water cooling; the annealing temperature is 700°C, the holding time is 24h, and the furnace is cooled to 500°C at 30°C / h and then air-cooled out of the furnace.

[0063] Among them, in step K, the ultra-fine process is one-time quenching + tempering.

[0064] Example 2

[0065] The steps for preparing sample 2 are as follows:

[0066] Step A, preparing the alloy according to the above element composition ratio, melting and homogenizing in a non-vacuum induction furnace, the melting temperature is 1520°C, and slag needs to be continuously added during the melting process for deoxidation and desulfurization, and 92% of the slag is removed after the material is cleared, and slag is added again to make slag, and an appropriate amount of Al powder is added for diffusion deoxidation, fully stirred and heated to 1580°C for sampling and analysis, and then heated to 1630°C, and the steel is tapped into the LF furnace;

[0067] Step B, after the ladle is placed in the LF station, the temperature is increased and the slag is adjusted. The composition is adjusted according to the sampling results of step A, and carbon powder, Al powder, and Si-Ca powder are added for diffusion deoxidation to maintain a reducing atmosphere. The slag white is sampled, and the temperature is increased to 1690°C to remove 65% of the slag and tap the steel into the VD station;

[0068] Step C, evacuate the VD furnace before placing 0.5kg / T of rare earth in the bag, the total evacuation time is 35min, the ultimate vacuum is 130Pa, the holding time is 12min, the temperature is measured after breaking the vacuum, argon is blown for 15min, and the temperature is measured at 1530℃ for steel pouring;

[0069] Step D: After pouring the electrode rod for 4 hours, the electrode rod is demoulded, slowly cooled to 300°C and immediately put into a furnace for annealing. After the annealing is completed, the ends of the electrode rod are flattened and the surface is polished;

[0070] Step E, placing the electrode rod processed in step D as an electrode in a protective atmosphere electroslag remelting furnace for secondary remelting and purification to form an electroslag ingot;

[0071] Step F, after the electroslag ingot is removed from the cover, it is loaded into the furnace for annealing within 24 hours, and after annealing, both ends of the electroslag ingot are flattened and the surface is polished;

[0072] Step G, placing the electroslag ingot treated in step F as an electrode in a vacuum consumable remelting furnace for remelting, purification, and degassing to form a consumable ingot;

[0073] Step H, the consumable ingot is taken out of the hood and air-cooled to 250°C, and then immediately put into the furnace for annealing. After the annealing is completed, the surface is polished and the next production process is transferred;

[0074] Step I: Place the steel ingot processed in step H in a heating furnace, heat it to 500°C at 82°C / h and keep it for 4 hours, then heat it to 850°C at 105°C / h and keep it for 6 hours, and finally heat it to 1280°C at 152°C / h and keep it for 35 hours, then open the furnace door and cool it to 1180°C and keep it for 1 hour before taking it out of the furnace for forging;

[0075] Step J: After forging, the mold is put into water for treatment. After water cooling, the mold is first returned to 550°C, then air-cooled to a surface temperature of 350°C and immediately put into a furnace for annealing. After annealing, flaw detection, flattening, and grinding are performed.

[0076] Step K: subjecting the module processed in step J to ultrafine processing to obtain the required material.

[0077] Among them, in step A, the molten steel is melted in a 20T non-vacuum induction furnace, and pre-slag is made by using a 3T furnace mixed blasting.

[0078] Wherein, in step B, the white slag is maintained for 32 minutes during the LF furnace refining period.

[0079] Among them, in step C, hydrogen needs to be measured after the VD furnace is broken.

[0080] In step D, the annealing temperature is 750° C., the holding time is 22 h, and the furnace is cooled to 500° C. at a rate of 28° C. / h and then air-cooled out of the furnace.

[0081] Among them, in step E, the protective atmosphere electroslag remelting uses 66 # Pre-melting slag, melting rate is 6.5kg / min, electroslag is finished, furnace cooling for 92 minutes and then hood cooling, hood cooling time is 73h.

[0082] In step F, the annealing temperature is 750° C., the holding time is 24 h, and the furnace is cooled to 500° C. at a rate of 28° C. / h and then air-cooled out of the furnace.

[0083] Among them, in step G, the maximum allowable arc current during the vacuum consumable remelting process is 15000±1000A, and the melting rate is 6.7kg / min.

[0084] In step H, the annealing temperature is 750° C., the holding time is 28 h, and the furnace is cooled to 500° C. at a rate of 28° C. / h and then air-cooled out of the furnace.

[0085] Among them, in step I, the forging process is one-piercing and one-pulling two-fire forming, and the starting forging temperature is 1052°C and the final forging temperature is 850°C.

[0086] Among them, in step J, the water cooling time is calculated based on the module thickness of 4min / 100mm, and air cooling is performed for 3min before water cooling; the annealing temperature is 750°C, the holding time is 25h, and the furnace is cooled to 500°C at 28°C / h and then air-cooled out of the furnace.

[0087] Among them, in step K, the ultra-fine process is one-time quenching + tempering.

[0088] Example 3

[0089] The preparation steps of sample 3 are as follows:

[0090] Step A, preparing the alloy according to the above element composition ratio, melting and homogenizing in a non-vacuum induction furnace, the melting temperature is 1515°C, and slag needs to be continuously added during the melting process for deoxidation and desulfurization, and 94% of the slag is removed after the material is cleared, and slag is added again to make slag, and an appropriate amount of Al powder is added for diffusion deoxidation, fully stirred, heated to 1570°C, sampled and analyzed, and then heated to 1625°C, and the steel is tapped into the LF furnace;

[0091] Step B, after the ladle is placed in the LF station, the temperature is increased and the slag is adjusted. The composition is adjusted according to the sampling results of step A, and carbon powder, Al powder, and Si-Ca powder are added for diffusion deoxidation to maintain a reducing atmosphere. The slag white is sampled, and the temperature is increased to 1680°C to remove 70% of the slag and tap the steel into the VD station;

[0092] Step C, evacuate the VD furnace before placing 0.5kg / T of rare earth in the bag, the total evacuation time is 38min, the ultimate vacuum is 130Pa, the holding time is 20min, the temperature is measured after breaking the vacuum, static argon is blown for 18min, and the temperature is measured at 1528℃ for steel pouring;

[0093] Step D: After 4 hours of casting, the electrode rod is demoulded, slowly cooled to 250°C and immediately put into a furnace for annealing. After annealing, the ends of the electrode rod are flattened and the surface is polished;

[0094] Step E, placing the electrode rod processed in step D as an electrode in a protective atmosphere electroslag remelting furnace for secondary remelting and purification to form an electroslag ingot;

[0095] Step F, after the electroslag ingot is removed from the cover, it is loaded into the furnace for annealing within 24 hours, and after annealing, both ends of the electroslag ingot are flattened and the surface is polished;

[0096] Step G, placing the electroslag ingot treated in step F as an electrode in a vacuum consumable remelting furnace for remelting, purification, and degassing to form a consumable ingot;

[0097] Step H, the consumable ingot is taken out of the hood and air-cooled to 220°C, and then immediately put into the furnace for annealing. After the annealing is completed, the surface is polished and the next production process is transferred;

[0098] Step I: Place the steel ingot processed in step H in a heating furnace, heat it to 500°C at 75°C / h and keep it for 4 hours, then heat it to 850°C at 95°C / h and keep it for 6 hours, finally heat it to 1280°C at 145°C / h and keep it for 35 hours, then open the furnace door and cool it to 1180°C and keep it for 1 hour before taking it out of the furnace for forging;

[0099] Step J: After forging, the mold is put into water for treatment. After water cooling, the mold is first returned to 550°C, then air-cooled to a surface temperature of 305°C and immediately put into a furnace for annealing. After annealing, flaw detection, flattening and grinding are performed.

[0100] Step K: subjecting the module processed in step J to ultrafine processing to obtain the required material.

[0101] Among them, in step A, the molten steel is melted in a 20T non-vacuum induction furnace, and pre-slag is made by using a 3T furnace mixed blasting.

[0102] Wherein, in step B, the white slag is maintained for 38 minutes during the LF furnace refining period.

[0103] Among them, in step C, hydrogen needs to be measured after the VD furnace is broken.

[0104] In step D, the annealing temperature is 730° C., the holding time is 25 h, and the furnace is cooled to 500° C. at a rate of 25° C. / h and then air-cooled out of the furnace.

[0105] Among them, in step E, the protective atmosphere electroslag remelting uses 66 # Pre-melting slag, melting rate is 6.8kg / min, electroslag is finished, furnace cooling for 100min and then hood cooling, hood cooling time is 76h.

[0106] In step F, the annealing temperature is 740° C., the holding time is 30 h, and the furnace is cooled to 500° C. at a rate of 25° C. / h and then air-cooled out of the furnace.

[0107] Among them, in step G, the maximum allowable arc current during the vacuum consumable remelting process is 15000±1000A, and the melting rate is 6.8kg / min.

[0108] In step H, the annealing temperature is 730° C., the holding time is 25 h, and the furnace is cooled to 500° C. at a rate of 25° C. / h and then air-cooled out of the furnace.

[0109] Among them, in step I, the forging process is one-piercing and one-pulling two-fire forming, and the starting forging temperature is 1060°C and the final forging temperature is 840°C.

[0110] Among them, in step J, the water cooling time is calculated based on the module thickness of 4min / 100mm, and air cooling is performed for 3min before water cooling; the annealing temperature is 730°C, the holding time is 25h, and the furnace is cooled to 500°C at 25°C / h and then air-cooled out of the furnace.

[0111] Among them, in step K, the ultra-fine process is one-time quenching + tempering.

[0112] Test Case

[0113] The inclusion levels of the mold steel materials produced in Examples 1-3 of the present invention were sampled and inspected according to the ASTM E45 standard rating chart microscopic inspection method for determining the content of non-metallic inclusions in steel grades. The samples of Examples 1-3 of the present invention all reached the levels shown in Table 2 below:

[0114] Table 2

[0115]

[0116] The organizational level of the obtained mold steel was sampled and inspected according to the SEP1614 hot working die steel microscopic inspection and evaluation standard rating chart microscopic inspection method, and it was found that all of them could reach SA1 level. The mesh level was sampled and inspected according to the GB / T1299 alloy tool steel standard rating chart microscopic inspection method, and it was found that all of them could reach level 1. The grain size level was rated according to the GB / T6394-2002 metal average grain size determination method, and it was found that all of them could reach level 10.

[0117] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

[0118] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other methods that can be understood by those skilled in the art.

Claims

1. A method for improving the purity and uniformity of mirror die steel, characterized in that: The mirror mold steel is composed of the following elements by weight percentage: C: 0.35-0.40%, Mn: 0.30-0.80%, Si: 0.70-1.00%, S: ≤0.003%, P: ≤0.025%, Cr: 13.00-14.00%, Ni: ≤0.50%, Mo: ≤0.50%, V: 0.25-0.35%, Cu: ≤0.20%, Al: ≤0.03%, and the balance is iron and unavoidable residual elements; the residual elements are: Ti: ≤0.008%, Nb: ≤0.01%, H: ≤0.0001%, O: ≤0.0015%, N: ≤0.01%; The method comprises the following steps: (1) preparing an alloy according to the above-mentioned element composition, melting it in a non-vacuum induction furnace at a melting temperature of 1510-1520° C., adding slag during the melting process for deoxidation and desulfurization, removing ≥90% of the slag after the material is cleared, then adding slag again to make slag, adding Al powder for diffusion deoxidation, heating to 1560-1580° C. for sampling and analysis, further heating to above 1620° C., tapping and entering an LF furnace; melting the molten steel in a 20T non-vacuum induction furnace, and pre-slag making using a 3T furnace mixed blasting; (2) After the ladle is placed in the LF station, the temperature is raised to adjust the slag, and the composition is adjusted according to the sampling results. Carbon powder, Al powder, and Si-Ca powder are added for diffusion deoxidation to maintain a reducing atmosphere. The slag is sampled, the temperature is raised to 1670-1690℃, and the slag is removed by ≥60%. The steel is then tapped into the VD station. The white slag retention time during the LF furnace refining period is ≥30min. (3) Before the VD furnace is evacuated, 0.5 kg / t of rare earth is placed in the bag. The total evacuation time is ≥30 min, the ultimate vacuum is ≤133 Pa, and the holding time is ≥10 min. After the vacuum is broken, the temperature is measured, and argon gas is blown for ≥10 min. The temperature is measured at 1525-1530 ° C, and the steel is poured; (4) The electrode rod is demoulded 4 hours after casting, slowly cooled to 200-300°C and then put into furnace for annealing. The annealing temperature is 700-750°C, the holding time is ≥20h, and the furnace is cooled to 500°C at a rate of ≤30°C / h and then air-cooled. After annealing, the ends of the electrode rod are flattened and the surface is polished. (5) The electrode rod is placed as an electrode in a protective atmosphere electroslag remelting furnace for secondary remelting and purification to form an electroslag ingot; protective atmosphere electroslag remelting uses 66 # Pre-melting slag, melting rate is 7.0~6.5kg / min, after electroslag is finished, furnace cooling ≥90min and then hood cooling, hood cooling time ≥72h; (6) After the electroslag ingot is removed from the cover, it is loaded into the furnace for annealing within 24 hours. After annealing, the two ends of the electroslag ingot are flattened and the surface is polished; the annealing temperature is 700-750°C, the holding time is ≥24h, and the furnace is cooled to 500°C at ≤30°C / h and then air-cooled out of the furnace; (7) placing the electroslag ingot as an electrode in a vacuum consumable remelting furnace for remelting, purification and degassing to form a consumable ingot; the maximum arc starting current during the vacuum consumable remelting process is 15000±1000A, and the melting rate is 6.7-7.0kg / min; (8) The consumable ingot is air-cooled to 150-250℃ and then put into furnace for annealing. After annealing, the surface is polished. The annealing temperature is 700-750℃, the holding time is ≥24h, and the ingot is cooled to 500℃ at a rate of ≤30℃ / h and then air-cooled. (9) The treated steel ingot is placed in a heating furnace, heated to 500°C at ≤80°C / h and kept at this temperature for 4 hours, then heated to 850°C at ≤100°C / h and kept at this temperature for 6 hours, and finally heated to 1280°C at ≤150°C / h and kept at this temperature for 35 hours, then the furnace door is opened to cool down to 1180°C and kept at this temperature for 1 hour before forging out of the furnace; the forging process is one-piercing and one-pulling two-fire forming, and the starting forging temperature is ≥1050°C, and the final forging temperature is 800-850°C; (10) After forging, water cooling is performed. After forging, the module is first returned to 550°C, and then air-cooled until the surface temperature reaches 250-350°C before being loaded into the furnace for annealing. After annealing, flaw detection, flattening, and grinding are performed. The water cooling time is calculated based on the module thickness of 4min / 100mm, and air cooling is performed for 3min before water cooling. The annealing temperature is 700-750°C, the holding time is ≥24h, and the furnace is cooled to 500°C at a rate of ≤30°C / h before being air-cooled. (11) The module processed in step (10) is subjected to ultra-fine processing. The ultra-fine processing includes one quenching and one tempering treatment to prepare a mirror mold steel with high purity and good structural uniformity.

Citation Information

Patent Citations

  • High-toughness and high-thermal-stability die steel and preparation method thereof

    CN114645200A

  • Mold material for injection molding of plastics and its production

    JP1989025950A