A hydrophobic fabric
By forming a lotus leaf-like micro-nano structure on the surface of the hydrophobic fabric, combining the cooperation of cotton yarn with PTFE yarn, and finishing the hydrophobic agent on the surface of the yarn, the problem of poor durability of the existing fabrics is solved, and the further development of the hydrophobic effect is achieved. Long-lasting hydrophobic effect and better washing resistance.
Patent Information
- Application Number
- CN202211665881.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-23
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-12-23
AI Technical Summary
During the washing process of existing hydrophobic fabrics, the finishing agent is prone to fall off, resulting in poor durability of the fabrics.
Using a single-layer or single-double-layer composite structure, a micro-nano structure similar to lotus leaves is formed on the surface of the fabric through long weft floating threads, combining the cooperation of cotton yarns with PTFE yarns, and finishing the hydrophobic agent on the surface of the yarn to form a durable hydrophobic film. layer.
It extends the hydrophobic aging of hydrophobic fabrics, improves the waterproof, anti-fouling and self-cleaning effects of the fabrics, and enhances the washing resistance of the fabrics.
Smart Images

Figure CN115821456B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of hydrophobic fabrics, and in particular to a hydrophobic fabric. Background Art
[0002] Superhydrophobic textile materials have the characteristics of being waterproof, antifouling and self-cleaning. They can be widely used in industrial waterproof fabrics, medical materials, protective clothing and self-cleaning materials, and have become one of the current research hotspots of functional textile materials. External surface energy is an intrinsic factor that affects the wettability of the material surface, which mainly depends on the composition elements of the material surface.
[0003] There are many super-hydrophobic phenomena in nature, such as the "self-cleaning effect" of lotus leaves. The surface of lotus leaves has a layer of long-chain olefin substances with low surface energy, and the surface is composed of regularly arranged papillae with micro-nano composite structures, which makes the lotus leaves reach super-hydrophobic properties. In order to improve the hydrophobic effect of fabrics, hydrophobic surface finishing is usually used on the surface of fabrics to improve the hydrophobic effect of the surface of fabrics.
[0004] According to the above-mentioned related technologies, when a hydrophobic surface finishing is performed on the surface of the fabric, the finishing agent is easily detached from the fabric during the washing process, causing the fabric to lose part of its hydrophobic effect, that is, there is a defect that the hydrophobic effect of the fabric is not durable. Summary of the invention
[0005] In order to improve the defect of poor water resistance and durability of fabrics, the present application provides a hydrophobic fabric and a weaving method thereof.
[0006] The present application provides a hydrophobic fabric, which adopts the following technical solution:
[0007] A hydrophobic fabric is composed of a single-layer tissue structure or a single-layer and double-layer composite tissue structure. The single-layer tissue structure is a tissue structure with protrusions. The single-layer composite tissue structure includes a single-layer tissue and a double-layer tissue. The single-layer tissue is a plain weave. The double-layer tissue is selected from five three-fly double-layer tissues or four irregular double-layer tissues.
[0008] By adopting the above technical scheme, a single-layer tissue utilizes the long weft floating lines of the fabric tissue to imitate a raised structure similar to the papillary structure of a lotus leaf. The raised structure is formed by the long weft floating lines floating on the surface of the fabric, forming a fine concave-convex effect on the surface of the fabric, that is, a micro-nano structure similar to a lotus leaf, so as to improve the surface hydrophobicity of the fabric. In addition, the raised structure produced by yarn weaving is not easy to lose its effectiveness during the washing process, thereby prolonging the hydrophobicity of the hydrophobic fabric.
[0009] The single- and double-layer composite structure utilizes five three-flies and four irregular weft satin weaves to form a combination of single and double layers, further increasing the specific surface area of the fabric. It not only forms a raised structure on the surface layer, forming a hydrophobic surface similar to a lotus leaf, but also improves the hydrophobic effect of the fabric.
[0010] Preferably, the protrusions in the single-layer tissue structure are selected from any one of circular protrusions, triangular protrusions, diamond-shaped protrusions, and square protrusions.
[0011] By adopting the above technical solution, a circular, triangular, diamond or square convex structure is formed on the surface of the fabric, a structure like a "hill" is formed on the surface of the fabric, air is stored in the concave part of the "hill", and an air layer is formed on the part close to the surface of the fabric, so that water droplets or dust cannot directly contact the fabric, thereby effectively improving the hydrophobic effect and self-cleaning property of the fabric.
[0012] Preferably, the single-layer tissue structure or the single-layer or double-layer composite tissue structure is made of yarn, and the yarn includes warp and weft, the warp is selected from cotton yarn with a count of 60 or 80, and the weft is PTFE yarn.
[0013] By adopting the above technical scheme, by combining cotton yarn with PTFE yarn, utilizing the excellent moisture absorption and breathability of cotton yarn and excellent comfort; and the excellent hydrophobic properties of PTFE yarn, the wearing experience of the fabric is improved while further improving the hydrophobic effect of the fabric.
[0014] Preferably, the surface layer is made of warp yarn, the yarn is yarn treated with a hydrophobic agent, and the hydrophobic agent includes nano-silica and poly (vinylidene fluoride-hexafluoropropylene) solution.
[0015] By adopting the above-mentioned technical scheme, in the technical scheme of the present application, a hydrophobic agent is preferably applied to the surface of the yarn, and the yarn is woven into a fabric. Compared with simply performing hydrophobic treatment on the surface of the fabric, the loading amount of the hydrophobic agent on the fabric is greatly increased, and the hydrophobic agent loaded on the yarn is not easy to fall off, which can extend the hydrophobic time of the fabric.
[0016] In this application, nano-silicon dioxide and poly (vinylidene fluoride-hexafluoropropylene) solution are used as hydrophobic agents. After nano-silicon dioxide is loaded on the surface of the yarn, it can give the surface of the yarn a relatively rough surface, which can further increase the micro-nano structure of the fabric surface, and after the poly (vinylidene fluoride-hexafluoropropylene) solution is wrapped outside the yarn, it can not only form a low surface energy surface outside the yarn, but also form a film to wrap the nano-silicon dioxide on the yarn. By coordinating low surface energy with rough micro-nano structure, the hydrophobic effect of the yarn is effectively improved, and by wrapping the nano-silicon dioxide with the film, the possibility of nano-silicon dioxide falling off is reduced, and the hydrophobic time of the yarn is extended.
[0017] Preferably, the preparation method for hydrophobic treatment comprises the following steps: taking nano-silica, 1H, 1H, 2H, 2H perfluorooctyl triethoxysilane and methyl trimethoxysilane in a mass ratio of 0.5: 2-8: 2; ultrasonically dispersing the nano-silica in anhydrous ethanol to obtain a dispersion, dropping 1H, 1H, 2H, 2H perfluorooctyl triethoxysilane and methyl trimethoxysilane into the dispersion, and continuing to stir to obtain an intermediate solution; immersing the yarn in the intermediate solution, taking it out, and drying it to obtain a dry yarn; then immersing the dry yarn in a poly (vinylidene fluoride - hexafluoropropylene) solution compatible with dimethylformamide, taking out the fiber, and drying it to obtain a hydrophobically treated yarn.
[0018] By adopting the above technical scheme, in the technical scheme of the present application, the nano-silica is modified in advance, and the nano-silica is wrapped and modified by 1H, 1H, 2H, 2H perfluorooctyltriethoxysilane and methyltrimethoxysilane, which not only introduces fluorine element into the nano-silica, improves the compatibility between the nano-silica and the poly (vinylidene fluoride-hexafluoropropylene) solution, and synergistically improves the hydrophobic effect and hydrophobic durability of the fabric; it also adjusts the particle size of the nano-silica to a certain extent, and the appropriate particle size can increase the roughness of the fabric surface, further improving the hydrophobic effect of the fabric.
[0019] In the technical solution of the present application, the ratio between nano-silica, 1H,1H,2H,2H perfluorooctyltriethoxysilane and methyltrimethoxysilane is optimized. The appropriate ratio makes the fluorine content loaded on the silica appropriate and the particle size appropriate, which can improve the surface roughness of the fabric, and the silica particles are not easy to fall off, thereby improving the hydrophobic effect of the fabric and prolonging the hydrophobic time of the fabric.
[0020] The present application adopts a two-step method to perform hydrophobic finishing on the yarn, thereby improving the convenience of the hydrophobic finishing and effectively improving the hydrophobic effect of the fabric.
[0021] Preferably, the hydrophobic fabric is a fabric that has been hydrophobically finished with a finishing agent, and the finishing agent includes 3-glycidyloxypropyltrimethoxysilane and polycarboxyl / methylsilsesquioxane nanospheres.
[0022] By adopting the above technical scheme, the technical scheme of the present application preferably adopts 3-glycidyloxypropyl trimethoxysilane and polycarboxyl / methyl silsesquioxane nanospheres to be arranged on the surface of the fabric, and the epoxy group in 3-glycidyloxypropyl trimethoxysilane is ring-opened, which can cross-link with the C-OH on the surface of the fabric, and at the same time, a large number of Si-OH groups are generated, which can react with the Si-OH groups on the surface of the polycarboxyl / methyl silsesquioxane nanospheres to dehydrate, thereby improving the durability fastness between the coating and the substrate. Therefore, the polycarboxyl / methyl silsesquioxane nanospheres can be firmly loaded on the surface of the fabric and form a micro-nano structure on the surface of the fabric, further improving the hydrophobic effect and hydrophobic time aging of the fabric.
[0023] Preferably, the hydrophobic finishing comprises the following steps: respectively taking 3-glycidyloxypropyltrimethoxysilane, polycarboxyl / methylsilsesquioxane nanospheres, and cross-linked aminosilicone emulsion, using a hydrolyzate of 3-glycidyloxypropyltrimethoxysilane and ethanol, immersing the fabric in the hydrolyzate, taking it out, drying, and obtaining a primary finishing product; immersing the primary finishing product in a polycarboxyl / methylsilsesquioxane nanosphere emulsion, taking it out, drying, and obtaining a secondary finishing product; and then immersing the secondary finishing product in a cross-linked aminosilicone emulsion, taking it out, drying, and shaping to obtain a hydrophobically finished fabric.
[0024] By adopting the above technical scheme, 3-glycidyloxypropyltrimethoxysilane, polycarboxyl / methylsilsesquioxane nanospheres, and cross-linked amino silicone emulsion in the technical scheme of the present application form a durable hydrophobic film layer on the surface of the fabric through layer-by-layer self-assembly, with the fabric as the film-forming matrix and the chemical bond Si-OH as the driving force.
[0025] The side chain of the cross-linked aminosilicone emulsion introduces Si-OH groups, which can cross-link with the other components in the finishing agent, which not only reduces the surface energy of the hydrophobic film layer, but also improves the density of the hydrophobic film layer. The hydrophobic effect of the fabric is further improved through the hydrophobic film layer, and a strong binding site is formed between the 3-glycidyloxypropyltrimethoxysilane and the fabric, which improves the bonding firmness between the hydrophobic film layer and the fabric and prolongs the hydrophobic time of the fabric.
[0026] The hydrophobic film layer can not only wrap the polycarboxyl / methylsilsesquioxane nanospheres, but also wrap the nano-silica on the surface of the yarn, thereby maintaining the roughness and hydrophobic effect of the fabric surface and prolonging the hydrophobic effect of the fabric.
[0027] Preferably, the mass fraction of 3-glycidyloxypropyltrimethoxysilane in the hydrolyzate is 0.5-0.8%, the solid content of the polycarboxyl / methylsilsesquioxane nanosphere emulsion is 0.5-1.5%, and the solid content of the cross-linked aminosilicone emulsion is 0.5-1.5%.
[0028] By adopting the above technical scheme, the mass fraction and solid content between the components in the finishing agent are optimized in the technical scheme of the present application. As the content of 3-glycidyl ether oxygen propyl trimethoxy silane increases, the binding site between the finishing agent and the fabric can be increased. After the appropriate content, the finishing site between the finishing agent and the fabric tends to be saturated. The appropriate content of polycarboxyl / methyl silsesquioxane nanospheres enables the nanospheres to form a uniform monolayer adsorption on the fabric surface, and it is not easy to stack, that is, the fabric surface obtains a uniform rough micro-nano structure to improve the hydrophobic effect of the fabric. Secondly, the appropriate content of cross-linked amino silicone emulsion, the cross-linked amino silicone emulsion can be oriented on the fabric surface, the hydrophilic groups such as amino and Si-OH groups can be oriented toward the fabric, and the hydrophobic Si-CH3 is oriented toward the hydrophobic film layer, which can form a uniform and dense and stable hydrophobic film layer, and the hydrophilic group is not easily exposed in the outermost layer, maintaining the excellent hydrophobic effect of the fabric.
[0029] Preferably, the fabric is loaded with a hydrophobic film, and the hydrophobic film is composed of titanium dioxide and polydimethylsiloxane.
[0030] By adopting the above technical solution, the technical solution of the present application preferably uses titanium dioxide and polydimethylsiloxane to form a hydrophobic film, titanium dioxide increases the surface roughness of the fabric, and then polydimethylsiloxane forms a film on the fabric surface and reduces the surface energy of the fabric, and the rough micro-nano structure and low surface energy are combined to effectively improve the hydrophobic effect of the fabric. In addition, the film formed by polydimethylsiloxane can fix nano titanium dioxide, reduce the possibility of nano titanium dioxide falling off, and maintain the hydrophobic durability of the fabric. In addition, the addition of titanium dioxide can effectively improve the UV resistance and self-cleaning effect of the fabric, reduce the number of times the fabric is washed, and further extend the hydrophobic time of the fabric.
[0031] Preferably, the method for preparing the hydrophobic film comprises the following steps: stirring and mixing titanium dioxide, polydimethylsiloxane and anhydrous ethanol to obtain a mixed solution, immersing the fabric in the mixed solution, taking it out, drying it, and performing plasma treatment to obtain the fabric loaded with the hydrophobic film.
[0032] Preferably, the amount of titanium dioxide used is 0.5-0.9 g / L, and the amount of polydimethylsiloxane used is 15-25 g / L.
[0033] By adopting the above technical scheme, in the technical scheme of the present application, after the hydrophobic film is loaded on the surface of the fabric, it is then treated with plasma, and the C-Si, Si-O bonds on the main chain and side chain of the polydimethylsiloxane long chain are reorganized and self-polymerized to exist in a more stable network structure. Therefore, the formed hydrophobic film can evenly cover the surface of the fabric, and open the CC and CO bonds on the fabric to form active sites of C· and O·, thereby enhancing the stability and firmness of the free radical polymerization of the fabric surface and polydimethylsiloxane, stably reducing the surface energy of the fabric, and improving the durability of titanium dioxide on the fabric, thereby effectively improving the hydrophobic effect and hydrophobic durability of the fabric.
[0034] The technical solution of the present application optimizes the dosage of each component in the hydrophobic film and the appropriate dosage of titanium dioxide, so that titanium dioxide can be uniformly adsorbed on the surface of the fabric in a single layer, thereby improving the surface hydrophobicity of the fabric. The appropriate dosage of polydimethylsiloxane allows the polydimethylsiloxane to react fully with the plasma, thereby improving the mechanical properties of the hydrophobic film, reducing the possibility of the hydrophobic film breaking and falling off, and improving the hydrophobic durability of the fabric.
[0035] In summary, this application has the following beneficial effects:
[0036] 1. Since the single-layer tissue structure in the present application utilizes the long floating warp threads of the fabric tissue to imitate a circular structure similar to the lotus leaf papillary structure, the long floating warp threads float on the fabric surface to form a circular convex structure, thereby forming a fine concave-convex effect on the fabric surface, that is, a micro-nano structure similar to a lotus leaf, so as to improve the surface hydrophobicity of the fabric, and the circular structure produced by yarn weaving is not easy to age during the washing process, thereby prolonging the hydrophobic time of the hydrophobic fabric.
[0037] By combining cotton yarn and PTFE yarn as the base layer, the cotton yarn has excellent moisture absorption and breathability, excellent comfort, and improves the wearing experience of the fabric while further improving the hydrophobic effect of the fabric.
[0038] 2. In the present application, it is preferred to apply a hydrophobic agent to the surface of the yarn, and the yarn is woven to obtain a fabric. Compared with simply applying a hydrophobic agent to the surface of the fabric, the amount of the hydrophobic agent loaded on the fabric is greatly increased, and the hydrophobic agent loaded on the yarn is not easy to fall off, which can extend the hydrophobic effect of the fabric. The loading of the hydrophobic agent increases the surface roughness of the yarn, reduces the surface energy of the yarn, and synergistically improves the hydrophobic effect and hydrophobic durability of the fabric.
[0039] 3. In the technical solution of this application, 3-glycidyloxypropyl trimethoxysilane, polycarboxyl / methyl silsesquioxane nanospheres, and cross-linked amino silicone emulsion are self-assembled layer by layer, with fabric as the film-forming matrix and chemical bond Si-OH as the driving force, to form a durable hydrophobic film on the surface of the fabric. Not only a dense hydrophobic film is formed, but also the bonding firmness between the hydrophobic film and the fabric is improved, maintaining the hydrophobic effect and hydrophobic durability of the fabric.
[0040] 4. In the present application, after the hydrophobic film is loaded on the surface of the fabric, it is then treated with plasma, so that the C-Si and Si-O bonds on the main chain and side chain of the polydimethylsiloxane long chain are reorganized and self-polymerized to exist in a more stable network structure. Therefore, the formed hydrophobic film can evenly cover the surface of the fabric, and open the CC and CO bonds on the fabric to form active sites of C· and O·, thereby enhancing the stability and firmness of the free radical polymerization of the fabric surface and polydimethylsiloxane, stably reducing the surface energy of the fabric, and improving the durability of titanium dioxide on the fabric, thereby effectively improving the hydrophobic effect, hydrophobic durability and self-cleaning effect of the fabric. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 It is the drawing diagram of Examples 1 and 18 of the present application;
[0042] Figure 2 It is the organization diagram and pattern diagram of Examples 1 and 18 of the present application;
[0043] Figure 3 It is the drawing diagram of Examples 2-3 and 19-20 of the present application;
[0044] Figure 4 is the organizational diagram of Examples 2 and 19 of the present application;
[0045] Figure 5 It is the pattern diagram of Example 2 of the present application;
[0046] Figure 6 is a table organization diagram of Examples 2 and 19 of the present application;
[0047] Figure 7 It is the organization diagram of Examples 2-3 and 19-20 of the present application;
[0048] Figure 8 is the organizational diagram of Examples 3 and 20 of the present application;
[0049] Fig. 9 It is the pattern diagram of Examples 3 and 20 of the present application;
[0050] Fig.10 It is a table organization diagram of Examples 3 and 20 of the present application. DETAILED DESCRIPTION
[0051] The present application is further described in detail below in conjunction with embodiments.
[0052] Preparation Example
[0053] Silicon dioxide preparation example
[0054] Preparation Example 1-3
[0055] Nano-silica, 1H, 1H, 2H, 2H perfluorooctyl triethoxysilane (HFOTES), and methyl trimethoxy silane (MTMS) were taken respectively, and the specific masses were shown in Table 1. The nano-silica was dispersed in 100 mL of anhydrous ethanol and ultrasonically dispersed for 10 min to obtain a dispersion. HFOTES was added to the dispersion, MTMS was added dropwise, and magnetic stirring was performed to obtain a hydrophobic nano-silica solution 1-3.
[0056] Table 1 Preparation Example 1-3 Dispersion Composition
[0057] content Preparation Example 1 Preparation Example 2 Preparation Example 3 Nano Silica 0.5g 0.5g 0.5g HFOTES 2mL 6mL 8mL MTMS 2mL 2mL 2mL
[0058] Example of hydrophobic yarn preparation
[0059] Preparation Example 4
[0060] Take the hydrophobic nano-silica solution 1, immerse the dry yarn in the hydrophobic nano-silica solution 1, take it out, dry it at room temperature for 12 hours, and dry it at 80°C for 1 hour to obtain the dry yarn, stir and mix 5g of poly(vinylidene fluoride-hexafluoropropylene) and 30mL of dimethylformamide (DMF) to obtain a spray liquid, spray the spray liquid onto the surface of the dry yarn, and dry it at 80°C for 1 hour to obtain the hydrophobic yarn 1.
[0061] Preparation Example 5-6
[0062] The difference from Preparation Example 4 is that: the hydrophobic nano-silica solution 2-3 is used to replace the hydrophobic nano-silica solution 1 in Preparation Example 4 to prepare the hydrophobic yarn 2-3.
[0063] Example
[0064] Example 1
[0065] The present application provides a hydrophobic fabric, which is composed of a single-layer tissue structure. The single-layer tissue structure is a tissue structure with protrusions, and the protrusions are circular protrusions.
[0066] The preparation method of the hydrophobic fabric comprises the following steps: Figure 1 and Figure 2The weaving is carried out on the machine according to the drafting diagram and organization diagram, wherein the warp yarn is 60S cotton single yarn, the weft yarn is 100D PTFE, the warp density is 663 pieces / 10cm, the weft density is 214 pieces / 10cm, the machine width is 21.6cm, four into one reed, the British reed number is 90, and the total number of warp roots (excluding the selvedge) is 1432.
[0067] The shape of the protrusion can be any one of round, square, triangle or diamond.
[0068] Example 2
[0069] The difference from Example 1 is that it is composed of a single-layer and double-layer composite tissue structure, which includes a single-layer tissue and a double-layer tissue, the single-layer tissue is a plain weave, and the double-layer tissue is selected from five three-fly woven double-layer tissues.
[0070] The preparation method of the hydrophobic fabric comprises the following steps: Figure 3-6 The warp yarn is 60S cotton single yarn, the weft yarn is 100D PTFE, the warp density is 649 pieces / 10cm, the weft density is 303 pieces / 10cm, the machine width is 22cm, four into one reed, the British reed number is 90, and the total number of warp roots (excluding the selvedge) is 1428.
[0071] Example 3
[0072] The difference from Example 1 is that it is composed of a single-layer and double-layer composite tissue structure, which includes a single-layer tissue and a double-layer tissue, the single-layer tissue is a plain weave, and the double-layer tissue is selected from five three-fly woven double-layer tissues.
[0073] The preparation method of the hydrophobic fabric comprises the following steps: Figure 3 , 7 -10's drafting diagram, pattern diagram, and machine diagram are used for weaving, wherein the warp yarn is 60S cotton single yarn, the weft yarn is 100D PTFE, the machine warp density is 799 yarns / 10cm, the machine weft density is 254 yarns / 10cm, the machine width is 22.8cm, four-in-one reed, the British reed number is 90, and the total number of warp roots (excluding the selvedge) is 1820.
[0074] Embodiment 4-6
[0075] The difference from Example 1 is that hydrophobic yarns 1-3 are used to replace the cotton yarn in Example 1 to prepare hydrophobic fabrics 4-6.
[0076] Example 7
[0077] The difference from Example 1 is that the fabric in Example 1 is subjected to hydrophobic finishing, and the hydrophobic finishing comprises the following steps: 3-glycidyloxypropyltrimethoxysilane (KH560), polycarboxyl / methylsilsesquioxane nanospheres (PCMSQNPs), and cross-linked aminosilicone emulsion (JASO) are taken, KH560 is mixed with ethanol, and a KH560 hydrolyzate with a mass fraction of 0.5% is prepared, and the hydrolyzate is adjusted to pH=6 with 10% acetic acid, and the fabric is immersed in the hydrolyzate for 20 seconds, taken out, and dried in an oven at 100°C for 10 minutes to obtain a primary finishing product, and the primary finishing product is immersed in PCMSQ with a solid content of 0.5%. The secondary finishing product was immersed in NPs emulsion for 1 min, taken out, and dried at 100°C for 10 min to obtain a secondary finishing product; the secondary finishing product was immersed in JASO emulsion with a solid content of 0.5% for 0.5 min, taken out, dried at 100°C for 10 min, and shaped at 160°C for 1 min to prepare a hydrophobic fabric 7.
[0078] Example 8
[0079] The difference from Example 7 is that: the hydrophobic fabric 8 is prepared by using KH560 hydrolyzate with a mass fraction of 0.7%.
[0080] Example 9
[0081] The difference from Example 7 is that: the hydrophobic fabric 9 is prepared by using KH560 hydrolyzate with a mass fraction of 0.8%.
[0082] Example 10
[0083] The difference from Example 7 is that the hydrophobic fabric 10 is prepared by using a PCMSQ NPs emulsion with a solid content of 1%.
[0084] Embodiment 11
[0085] The difference from Example 7 is that the hydrophobic fabric 11 is prepared by using a PCMSQ NPs emulsion with a solid content of 1.5%.
[0086] Example 12
[0087] The difference from Example 7 is that the hydrophobic fabric 12 is prepared by using a JASO emulsion with a solid content of 1%.
[0088] Embodiment 13
[0089] The difference from Example 7 is that the hydrophobic fabric 13 is prepared by using a JASO emulsion with a solid content of 1.5%.
[0090] Embodiment 14
[0091] The difference from Example 5 is that the fabric in Example 5 is subjected to hydrophobic finishing, and the hydrophobic finishing comprises the following steps: 3-glycidyloxypropyltrimethoxysilane (KH560), polycarboxyl / methylsilsesquioxane nanospheres (PCMSQNPs), and cross-linked aminosilicone emulsion (JASO) are taken, KH560 is mixed with ethanol, and a KH560 hydrolyzate with a mass fraction of 0.7% is prepared, and the hydrolyzate is adjusted to pH=6 with 10% acetic acid, and the fabric is immersed in the hydrolyzate for 20 seconds, taken out, and dried in an oven at 100°C for 10 minutes to obtain a primary finishing product, and the primary finishing product is immersed in PCMSQ with a solid content of 1%. The fabric was immersed in NPs emulsion for 1 min, taken out, and dried at 100°C for 10 min to obtain a secondary finished product. The secondary finished product was immersed in JASO emulsion with a solid content of 1% for 0.5 min, taken out, dried at 100°C for 10 min, and fixed at 160°C for 1 min to prepare a hydrophobic fabric 14.
[0092] Examples 15-17
[0093] The difference from Example 1 is that the surface of the fabric is loaded with a hydrophobic film, and the preparation method of the hydrophobic film comprises the following steps: titanium dioxide and polydimethylsiloxane (PDMS) are taken separately, the specific masses are shown in Table 2, dispersed in anhydrous ethanol, ultrasonically oscillated to obtain a mixed solution, and the fabric is immersed in the mixed solution. After 2 minutes, it is taken out, dried, and placed in a plasma treatment box under air environment, the power is 550 W, the plate spacing is 4.5 mm, and the time is 90 s to prepare hydrophobic fabrics 15-17.
[0094] Table 2 Composition of dispersions of Examples 1-3
[0095]
[0096]
[0097] Embodiment 18
[0098] The present application provides a hydrophobic fabric, which is composed of a single-layer tissue structure. The single-layer tissue structure is a tissue structure with protrusions, and the protrusions are circular protrusions.
[0099] The preparation method of the hydrophobic fabric comprises the following steps: Figure 1 and Figure 2 The weft yarn is 100D PTFE, the warp density is 657 yarns / 10cm, the weft density is 236 yarns / 10cm, the width is 21.8cm, four-in-one reed, the British reed number is 100, and the total number of warp roots (excluding the selvedge) is 1432.
[0100] Embodiment 19
[0101] The difference from Example 1 is that it is composed of a single-layer and double-layer composite tissue structure, which includes a single-layer tissue and a double-layer tissue, the single-layer tissue is a plain weave, and the double-layer tissue is selected from five three-fly woven double-layer tissues.
[0102] The preparation method of the hydrophobic fabric comprises the following steps: Figure 3-6 The warp yarn is 80S cotton single yarn, the weft yarn is 100D PTFE, the warp density is 655 pieces / 10cm, the weft density is 314 pieces / 10cm, the machine width is 21.8cm, four into one reed, the British reed number is 100, and the total number of warp roots (excluding the selvedge) is 1428.
[0103] Embodiment 20
[0104] The difference from Example 1 is that it is composed of a single-layer and double-layer composite tissue structure, which includes a single-layer tissue and a double-layer tissue, the single-layer tissue is a plain weave, and the double-layer tissue is selected from five three-fly woven double-layer tissues.
[0105] The preparation method of the hydrophobic fabric comprises the following steps: Figure 3 , 7 -10's drafting diagram, pattern diagram, organization diagram, etc. are used for weaving, wherein the warp yarn is 80S cotton single yarn, the weft yarn is 100D PTFE, the warp density is 802 yarns / 10cm, the weft density is 341 yarns / 10cm, the machine width is 22.7cm, four-in-one reed, the British reed number is 100, and the total number of warp roots (excluding the selvedge) is 1784.
[0106] Comparative Example
[0107] Comparative Example 1
[0108] The difference between this comparative example and Example 1 is that the fabric in this comparative example is a plain fabric without protrusions, and a hydrophobic fabric 21 is obtained.
[0109] Comparative Example 2
[0110] The difference between this comparative example and Example 1 is that in this comparative example, hydrophobic finishing is directly performed on the surface of the fabric to obtain the hydrophobic fabric 22.
[0111] Comparative Example 3
[0112] The difference between this comparative example and Example 1 is that in this comparative example, a hydrophobic film is directly loaded on the surface of the fabric to obtain a hydrophobic fabric 23.
[0113] Performance testing
[0114] (1) Contact angle: The contact angle was measured using a contact angle meter. The droplet volume was 5 μL and the photographing time was 60 s. Each group of samples was tested 5 times and the average value was taken.
[0115] (2) Adhesion performance test: The fabric samples were cut into 5 cm × 10 cm and washed using the 1A method in AATCC61-2007 “Color Fastness to Washing: Accelerated”. After washing 100 times, the hydrophobicity was tested again.
[0116] (3) Air permeability test: GB / T 5453-1997 “Test method for air permeability of textile fabrics”, test the air permeability of the fabrics in Examples 1-3 and Examples 18-20.
[0117] (4) Moisture permeability test: With reference to GB / T12704.1-2009 “Test method for moisture permeability of textile fabrics - Part 1: Moisture absorption method”, the moisture permeability of the fabrics in Examples 1-3 and Examples 18-20 was tested.
[0118] Table 3 Performance test of Examples 1-17 and Comparative Examples 1-3
[0119]
[0120]
[0121] Table 3 Performance test of Examples 1-17 and Comparative Examples 1-3
[0122]
[0123] By referring to the performance test comparison in Table 7, we can find that:
[0124] (1) By comparing Examples 1-3 with Comparative Examples 1-3, it can be found that the waterproof performance and washing resistance of the hydrophobic fabrics prepared in Examples 1-3 are improved. This indicates that the surface layer of the present application utilizes the long weft floating lines of the fabric tissue to imitate a circular structure similar to the lotus leaf papilla structure, and the long weft floating lines float on the fabric surface to form a circular convex structure, thereby forming a fine concave-convex effect on the fabric surface, that is, a micro-nano structure similar to a lotus leaf, so as to improve the surface hydrophobicity of the fabric, and the circular structure produced by yarn weaving is not easy to lose its effectiveness during the washing process, thereby prolonging the hydrophobic effect of the hydrophobic fabric.
[0125] (2) By comparing Examples 4-6 with Example 1, it can be found that the waterproof performance and washing resistance of the hydrophobic fabrics prepared in Examples 4-6 are improved. This shows that the present application can effectively improve the hydrophobic effect of the yarn by combining low surface energy with rough micro-nano structure, and by wrapping the nano-silica with a thin film, the possibility of nano-silica falling off is reduced, thereby extending the hydrophobic effect of the yarn.
[0126] (3) By comparing Examples 7-9, 10-11, 12-13, and 14 with Example 1, it can be found that the waterproof performance and washing resistance of the hydrophobic fabrics prepared in Examples 7-14 are improved, which shows that the present application uses KH560, PCMSQ NPs, and JASO to form a durable hydrophobic film layer on the surface of the fabric through layer-by-layer self-assembly, with the fabric as the film-forming matrix and the chemical bond Si-OH as the driving force. KH560 increases the binding sites between the hydrophobic film layer and the fabric, and stably improves the hydrophobic durability of the fabric. The present application optimizes the mass fraction or solid content of KH560, PCMSQ NPs, and JASO, so that the nanospheres in the hydrophobic film layer are uniformly adsorbed on the surface of the fabric, the binding sites between the hydrophobic film layer and the fabric are appropriate, and the hydrophobic groups can be evenly arranged outside the fabric, so that the fabric obtains an excellent hydrophobic effect.
[0127] (4) By comparing Examples 15-17 with Example 1, it can be found that the waterproof performance and washing resistance of the hydrophobic fabrics prepared in Examples 15-17 are improved. This shows that the present application adopts a method of loading a hydrophobic film on the surface of the fabric and then performing plasma treatment, so that the beads in the long chain of polydimethylsiloxane and the C-Si, Si-O bonds on the side chain are reorganized and self-polymerized to exist in a more stable network structure. Therefore, the formed hydrophobic film can evenly cover the surface of the fabric, open the CC and CO bonds on the fabric, form active sites of C· and O·, enhance the stability and firmness of the free radical polymerization of the fabric surface and polydimethylsiloxane, stably reduce the surface energy of the fabric, and improve the durability of titanium dioxide on the fabric, effectively improving the hydrophobic effect and hydrophobic durability of the fabric.
[0128] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A hydrophobic fabric, characterized in that: It is composed of a single-layer tissue structure or a single-layer and double-layer composite tissue structure, wherein the single-layer tissue structure is a tissue structure with convexities, and the single-layer and double-layer composite tissue structure includes a single-layer tissue and a double-layer tissue, wherein the single-layer tissue is a plain weave, and the double-layer tissue is selected from five three-layer double-layer tissues or four irregular double-layer tissues; The single-layer tissue structure or the single-layer and double-layer composite tissue structure is made of yarn, and the yarn is a yarn treated with a hydrophobic agent, and the hydrophobic agent includes nano-silicon dioxide and poly (vinylidene fluoride-hexafluoropropylene) solution; The hydrophobic treatment comprises the following steps: taking nano silicon dioxide, 1H, 1H, 2H, 2H perfluorooctyl triethoxysilane and methyl trimethoxysilane in a mass ratio of 0.5:(2-8):2; ultrasonically dispersing the nano silicon dioxide in anhydrous ethanol to obtain a dispersion, dropping 1H, 1H, 2H, 2H perfluorooctyl triethoxysilane and methyl trimethoxysilane into the dispersion, and continuously stirring to obtain an intermediate solution; immersing the yarn in the intermediate solution, taking it out, and drying it to obtain a dry yarn; then immersing the dry yarn in a poly(vinylidene fluoride-hexafluoropropylene) solution prepared by mixing poly(vinylidene fluoride-hexafluoropropylene) and dimethylformamide, taking out the fiber, and drying it to obtain a hydrophobic treated yarn; The hydrophobic fabric is a fabric that has been hydrophobically finished with a finishing agent, and the finishing agent includes 3-glycidyloxypropyltrimethoxysilane and polycarboxyl / methylsilsesquioxane nanospheres; The hydrophobic finishing comprises the following steps: taking 3-glycidyloxypropyl trimethoxysilane, polycarboxyl / methyl silsesquioxane nanospheres and cross-linked amino silicone emulsion respectively, mixing 3-glycidyloxypropyl trimethoxysilane with ethanol to obtain a hydrolyzate, immersing the fabric in the hydrolyzate, taking it out, drying it, and obtaining a primary finishing product, immersing the primary finishing product in a polycarboxyl / methyl silsesquioxane nanosphere emulsion, taking it out, drying it, and obtaining a secondary finishing product; and then immersing the secondary finishing product in a cross-linked amino silicone emulsion, taking it out, drying it, and shaping it to obtain a hydrophobically finished fabric.
2. The hydrophobic fabric according to claim 1, characterized in that: The protrusions in the single-layer tissue structure are selected from any one of circular protrusions, triangular protrusions, diamond-shaped protrusions, and square protrusions.
3. The hydrophobic fabric according to claim 1, characterized in that: The yarn comprises a warp and a weft, wherein the warp is selected from cotton yarn with a count of 60 or 80, and the weft is PTFE yarn.
4. The hydrophobic fabric according to claim 1, characterized in that: The mass fraction of 3-glycidyloxypropyltrimethoxysilane in the hydrolyzate is 0.5-0.8%, the solid content of the polycarboxyl / methylsilsesquioxane nanosphere emulsion is 0.5-1.5%, and the solid content of the cross-linked aminosilicone emulsion is 0.5-1.5%.
5. The hydrophobic fabric according to claim 1, characterized in that: The fabric is loaded with a hydrophobic film, which is composed of titanium dioxide and polydimethylsiloxane.
6. The hydrophobic fabric according to claim 5, characterized in that: The preparation method of the hydrophobic film comprises the following steps: mixing titanium dioxide, polydimethylsiloxane and anhydrous ethanol by stirring to obtain a mixed solution, immersing fabric in the mixed solution, taking out, drying, and performing plasma treatment to obtain fabric loaded with the hydrophobic film.
Citation Information
Patent Citations
Preparation method of super-hydrophobic cellulose material with micro-nano structure
CN103938432A
Hydrophobic, breathable, antibacterial and skin-friendly bib fabric and preparation method thereof
CN105951442A