A method for preparing a nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material

Through the preparation method of nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material, the problems of poor cycle stability and high energy consumption of silicon oxide materials are solved, and the high energy density and electrochemical performance of lithium-ion batteries are improved. .

CN115832263BActive Publication Date: 2024-11-15GUANGZHOU UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211679790.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-26
Publication Date
2024-11-15
Estimated Expiration
2042-12-26

AI Technical Summary

Technical Problem

The cycling stability of the silicon oxide negative electrode materials in existing lithium-ion batteries is poor, the energy consumption is high and the safety risks are high, and it cannot meet the growing energy density requirements of lithium-ion batteries.

Method used

The preparation method of nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material is adopted. By mixing silicon oxide with alkali metal compounds, the phosphorus source is dispersed at low temperature and in situ polymerization is carried out to form nitrogen and phosphorus Co-doped carbon structure reduces disproportionation temperature and improves conductivity.

Benefits of technology

It realizes the low energy consumption, safe and reliable preparation of nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material with high first-term efficiency and high cycle stability, and improves the energy density and electrochemical performance of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115832263B_ABST
    Figure CN115832263B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of negative electrode materials for lithium ion batteries, and in particular to a method for preparing a nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material. The method comprises the following steps: mixing silicon oxide with an alkali metal compound and / or an alkaline earth metal compound by ball milling, and heat treating the mixture under a protective atmosphere to obtain modified silicon oxide; dispersing the modified silicon oxide in a phosphorus source solution at a low temperature, and then adding a nitrogen-containing carbon source to mix to obtain a solution A; adding an oxidant to the phosphorus source solution, stirring evenly to obtain a solution B, and adding the solution B to the solution A to perform an in-situ polymerization reaction; washing and drying the obtained product, and then heat treating it under a protective atmosphere, and grinding and crushing to obtain a nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material. The preparation method has low energy consumption, is safe and reliable, and the prepared nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material has excellent conductivity and excellent electrochemical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of negative electrode materials for lithium ion batteries, and in particular to a method for preparing a nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material. Background Art

[0002] Lithium-ion batteries have the characteristics of high energy density, long life, and environmental friendliness. They are one of the most attractive energy storage devices today and play an increasingly important role in modern society. However, to date, most commercial lithium-ion batteries use graphite as the negative electrode material, with a theoretical specific capacity of 372mAh / g, which cannot meet the growing energy density requirements of lithium-ion batteries. Among the emerging negative electrode materials for lithium-ion batteries, silicon-based negative electrode materials are considered to be the most promising materials to replace graphite. The theoretical capacity of single silicon material is as high as 4200mAh / g, which is nearly ten times that of graphite. Single silicon has the advantages of relatively low delithiation potential (0.4V), environmental friendliness, and abundant resources. However, single silicon also has disadvantages such as high production cost, large volume expansion change, and low intrinsic conductivity.

[0003] Relatively speaking, the theoretical capacity of silicon oxide is only 2100mAh / g, but the volume change is small during the lithiation process. Silicon oxide is also considered to be a very promising substitute for elemental Si because of its low cost and easy synthesis. However, the volume expansion problem of silicon oxide will still lead to the crushing of active materials, electrode disintegration, and the continuous rupture and formation of solid electrolyte interface film (SEI), and the above problems will eventually manifest as poor cycle stability. In addition, due to the presence of active oxygen, silicon oxide materials will consume part of the lithium ions in the battery, resulting in an increase in the irreversible capacity of silicon oxide and a reduction in its first coulombic efficiency. The intrinsic conductivity of silicon oxide negative electrode materials is also relatively low, resulting in poor rate performance. These factors jointly restrict the large-scale application of silicon oxide negative electrodes in lithium-ion batteries.

[0004] The prior art requires pretreatment of silicon oxide before using silicon oxide negative electrode materials to remove part of the active oxygen in silicon oxide, and combines carbon coating treatment to improve the cycle stability of battery materials. Chinese invention patent CN114249329A provides a silicon oxide composite material and a preparation method thereof to improve the initial coulombic efficiency and conductivity of silicon oxide. The method is to preheat the silicon oxide raw material so that part of the silicon oxide raw material undergoes a disproportionation reaction; continuously introduce protective gas and carbon source gas, and perform chemical vapor deposition on the preheated silicon oxide raw material. The method uses a conventional high-temperature disproportionation reaction, but the temperature required for the silicon oxide disproportionation reaction is relatively high, generally above 850°C, and the disproportionation effect is not obvious. As the disproportionation temperature and time increase, the disproportionation effect becomes more obvious, but the required energy consumption increases.

[0005] Chinese invention patent CN114014325A discloses a method for preparing porous silicon negative electrode materials by magnesium thermal reduction, which uses magnesium powder to reduce silicon oxide and prepare porous silicon, and then uses an organic carbon source to pyrolyze and carbonize the porous silicon at high temperature to prepare a porous silicon / carbon composite material. This method uses magnesium thermal reduction to consume active oxygen, and magnesium thermal reaction is a highly exothermic reaction, which may pose a safety hazard during high-temperature firing and has a high cost.

[0006] Therefore, there is an urgent need for a method for preparing nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode materials that has low energy consumption, is safe and reliable, and can prepare high initial efficiency and high cycle stability. Summary of the invention

[0007] The first purpose of the present invention is to provide a method for preparing a nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material. The method has low energy consumption, safety and reliability. At the same time, the prepared nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material has high initial efficiency and high cycle stability.

[0008] The second object of the present invention is to provide a nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material, aiming to meet the ever-increasing energy density requirements of lithium-ion batteries.

[0009] The present invention provides a method for preparing a nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material, comprising the following steps:

[0010] (1) ball-milling silicon dioxide and a metal compound to obtain a mixture, and subjecting the mixture to a heat treatment reaction under a protective atmosphere to obtain modified silicon dioxide; the metal compound is an alkali metal compound and / or an alkaline earth metal compound;

[0011] (2) dispersing the modified silicon dioxide obtained in step (1) in a phosphorus source solution at low temperature, and then adding a nitrogen-containing carbon source, and mixing to obtain a solution A;

[0012] (3) taking a new phosphorus source solution, adding an oxidant thereto, stirring evenly to obtain a solution B, and adding the solution B to the solution A obtained in step (2) to carry out an in-situ polymerization reaction;

[0013] (4) The product obtained by the in-situ polymerization reaction in step (3) is washed and dried, and then subjected to a heat treatment reaction under a protective atmosphere, and then ground and pulverized to obtain a nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material.

[0014] Preferably, the metal compound in step (1) is one or more of sodium carbonate, lithium carbonate, potassium carbonate, calcium carbonate, sodium hydroxide, potassium hydroxide, lithium hydroxide, aluminum oxide, magnesium oxide, and sodium citrate, preferably sodium carbonate. The mass ratio of silicon dioxide to the metal compound in step (1) is 1:0.01-0.8, more preferably 1:0.2-0.5. Silicon dioxide is preferably amorphous silicon dioxide of 200 mesh.

[0015] Preferably, the reaction temperature of the heat treatment reaction in step (1) is 750-900°C, the reaction time is 1-24h, and the heating rate is 1-10°C / min. More preferably, the reaction temperature is 850°C.

[0016] Preferably, the low temperature in step (2) is 0-5°C, preferably 0-2°C.

[0017] Preferably, the phosphorus source solutions in step (2) and step (3) are one or more of phosphoric acid, phytic acid, hypophosphorous acid, and phosphorous acid, and the concentration of the phosphorus source solution is 0.5M-5M, more preferably 1-3M.

[0018] Preferably, in step (2), the nitrogen-containing carbon source is aniline monomer and / or pyrrole monomer, and the amount of the nitrogen-containing carbon source added is 1-10 times the amount of the modified silicon oxide added.

[0019] When the amount of modified silicon dioxide added in step (2) is 0.1-1 g, the volume of the phosphorus source solution is 10-100 ml; at this time, the volume of the phosphorus source solution in step (3) is 10-50 ml.

[0020] Preferably, the oxidant in step (3) is one of ammonium persulfate, potassium persulfate, H2O2, and CuCl2, more preferably aniline monomer, and the molar ratio of the oxidant in step (3) to the nitrogen-containing carbon source in step (2) is 1:1-5.

[0021] Preferably, the reaction time of the in-situ polymerization reaction in step (3) is 3-24 h, more preferably 6-24 h.

[0022] Preferably, the reaction temperature of the heat treatment reaction in step (4) is 750-900°C, the reaction time is 1-10h, and the heating rate is 5-10°C / min.

[0023] Preferably, the protective atmosphere in step (1) and step (4) is one or two of helium, neon, argon and nitrogen, more preferably nitrogen and / or argon.

[0024] The present invention also provides a nitrogen and phosphorus co-doped carbon-coated modified silicon 2 Oxide negative electrode material prepared by the above preparation method.

[0025] Beneficial effects:

[0026] In the preparation method of the nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material provided by the present invention, the addition of alkali metal compounds and / or alkaline earth metal compounds promotes the formation of elemental Si and SiO2 from silicon oxide, and a part of the active oxygen in silicon oxide is converted into lithium-inactive SiO2, thereby improving the first coulombic efficiency of the material; at the same time, the disproportionation temperature is lowered, the energy consumption is reduced, and the disproportionation effect is better than that of high-temperature thermal disproportionation reaction; the alkali metal compounds and / or alkaline earth metal compounds have low requirements for storage conditions and are suitable for most industrial production conditions.

[0027] The in-situ polymerization method adopted by the present invention allows carbon materials to grow on the surface of the material to form a three-dimensional conductive network carbon structure, which improves the conductivity of the battery material, prevents the electrolyte from penetrating into the interior of the material, reduces the formation of the SEI film, and can inhibit the volume expansion of silicon oxide.

[0028] The present invention adopts nitrogen and phosphorus co-doping, wherein nitrogen doping is beneficial to ion conduction, improves the Fermi level of carbon atoms, and ultimately improves the electronic conductivity of the negative electrode material; phosphorus doping can provide more flat layer space for the carbon layer, induce more defect sites, and enhance the electrode material and Li + The interaction between the two is beneficial to ion diffusion; the combination of the two makes the nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material prepared by the present invention have excellent conductivity and excellent electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a scanning electron microscope image of the modified silicon dioxide material obtained in Example 1;

[0030] Figure 2 This is a scanning electron microscope image of the nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material obtained in Example 1;

[0031] Figure 3 This is a transmission electron micrograph of the nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material obtained in Example 1;

[0032] Figure 4 This is the XRD pattern of the nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material obtained in Example 1;

[0033] Figure 5 The first charge-discharge curve of the nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material obtained in Example 1;

[0034] Figure 6 The cycle performance diagram of the nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material obtained in Example 1;

[0035] Figure 7 The rate performance diagram of the nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material obtained in Example 1;

[0036] Figure 8 The cycle performance diagram of the nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material obtained in Example 2;

[0037] Fig. 9 The cycle performance diagram of the nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material obtained in Example 3;

[0038] Fig.10 The first charge-discharge curve of the nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material obtained in Example 4;

[0039] Fig.11 The cycle performance diagram of the nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material obtained in Example 4;

[0040] Fig.12 This is the cycle performance diagram of the nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material obtained in Example 5. DETAILED DESCRIPTION

[0041] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.

[0042] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form also includes the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this description, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0043] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0044] Example 1

[0045] A method for preparing a nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material comprises the following steps:

[0046] (1) ball-milling 200-mesh amorphous silicon dioxide and sodium carbonate in a mass ratio of 1:0.05 to obtain a mixture, and heat-treating the mixture at 850° C. for 12 h in a nitrogen atmosphere to obtain modified silicon dioxide;

[0047] (2) At 0° C., 0.4 g of the modified silicon dioxide obtained in step (1) was dispersed in 20 ml of a 1 M phosphoric acid solution, and then 0.4 g of aniline monomer was added and mixed to obtain a solution A;

[0048] (3) Re-take 20 ml of 1 M phosphoric acid solution, add oxidant ammonium persulfate thereto, the molar ratio of ammonium persulfate to aniline monomer added in step (2) is 1:1, stir evenly until colorless and transparent, obtain solution B, slowly drip solution B into solution A obtained in step (2), and carry out in-situ polymerization reaction for 6 hours; the polymerization reaction of aniline is a strongly exothermic reaction, first prepare solution B of oxidant ammonium persulfate, and then slowly drip it into solution A, which effectively avoids sudden change of reaction temperature and makes the reaction more complete.

[0049] (4) The product obtained by the in-situ polymerization reaction in step (3) is filtered, washed, and dried, and then sent into a tubular furnace. The temperature is increased to 900° C. at a heating rate of 5° C. / min under a protective nitrogen atmosphere and calcined for 3 h. After natural cooling, the product is ground and pulverized to obtain a nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material.

[0050] The scanning electron microscope image of the modified silicon dioxide material obtained in Example 1 is as follows: Figure 1 As shown in the figure, it can be seen that the surface of silicon oxide modified with sodium carbonate is relatively smooth and the particle size has hardly changed. This shows that the modification of silicon oxide with sodium carbonate does not significantly change the morphology, but mainly changes the internal structure.

[0051] The scanning electron microscope image of the nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material obtained in Example 1 is as follows Figure 2 As shown in the figure, it can be seen that the modified silicon oxide is dispersed in the carbon source, which can effectively alleviate the volume expansion of silicon oxide during the cycle process and improve the electrochemical stability.

[0052] The transmission electron microscopy image of the nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material obtained in Example 1 is as follows Figure 3 As shown in the figure, the original silicon oxide is an amorphous structure, and no lattice fringes can be seen under a transmission electron microscope. However, after adding sodium carbonate, lattice fringes of single crystal silicon and silicon dioxide can be observed, which shows that the addition of sodium carbonate can promote the disproportionation of amorphous silicon oxide into silicon and silicon dioxide.

[0053] The XRD pattern of the nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material obtained in Example 1 is as follows: Figure 4 As shown, the carbon in the final material is amorphous carbon, so there is no characteristic peak of carbon in XRD, but the characteristic peaks of silicon and silicon dioxide can be clearly seen, which further illustrates that the addition of sodium carbonate can promote the disproportionation of amorphous silicon oxide into silicon element and silicon dioxide.

[0054] Example 2

[0055] A method for preparing a nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material comprises the following steps:

[0056] (1) ball-milling 200-mesh amorphous silicon dioxide and sodium carbonate in a mass ratio of 1:0.05 to obtain a mixture, and heat-treating the mixture at 850° C. for 12 h in a nitrogen atmosphere to obtain modified silicon dioxide;

[0057] (2) At 0° C., 0.4 g of the modified silicon dioxide obtained in step (1) was dispersed in 20 ml of a 1 M phosphoric acid solution, and then 0.8 g of aniline monomer was added and mixed to obtain a solution A;

[0058] (3) Re-take 20 ml of 1 M phosphoric acid solution, add oxidant ammonium persulfate thereto, the molar ratio of ammonium persulfate to aniline monomer added in step (2) is 1:1, stir evenly until colorless and transparent, obtain solution B, add solution B to solution A obtained in step (2), and carry out in-situ polymerization for 6 hours; the polymerization reaction of aniline is a strongly exothermic reaction, first prepare solution B of oxidant ammonium persulfate, and then slowly add it dropwise to solution A, which effectively avoids sudden change in reaction temperature and makes the reaction more complete.

[0059] (4) The product obtained by the in-situ polymerization reaction in step (3) is filtered, washed, and dried, and then sent into a tubular furnace. The temperature is increased to 900° C. at a heating rate of 5° C. / min under a protective nitrogen atmosphere and calcined for 3 h. After natural cooling, the product is ground and pulverized to obtain a nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material.

[0060] Example 3

[0061] A method for preparing a nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material comprises the following steps:

[0062] (1) ball-milling 200-mesh amorphous silicon dioxide and sodium carbonate in a mass ratio of 1:0.1 to obtain a mixture, and heat-treating the mixture at 850° C. for 12 h in a nitrogen atmosphere to obtain modified silicon dioxide;

[0063] (2) At 0° C., 0.4 g of the modified silicon dioxide obtained in step (1) was dispersed in 20 ml of a 1 M phosphoric acid solution, and then 0.4 g of aniline monomer was added and mixed to obtain a solution A;

[0064] (3) Re-take 20 ml of 1 M phosphoric acid solution, add oxidant ammonium persulfate thereto, the molar ratio of ammonium persulfate to aniline monomer added in step (2) is 1:1, stir evenly until colorless and transparent, obtain solution B, add solution B to solution A obtained in step (2), and carry out in-situ polymerization for 6 hours; the polymerization reaction of aniline is a strongly exothermic reaction, first prepare solution B of oxidant ammonium persulfate, and then slowly add it dropwise to solution A, which effectively avoids sudden change in reaction temperature and makes the reaction more complete.

[0065] (4) The product obtained by the in-situ polymerization reaction in step (3) is filtered, washed, and dried, and then sent into a tubular furnace. The temperature is increased to 900° C. at a heating rate of 5° C. / min under a protective nitrogen atmosphere and calcined for 3 h. After natural cooling, the product is ground and pulverized to obtain a nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material.

[0066] Example 4

[0067] A method for preparing a nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material comprises the following steps:

[0068] (1) ball-milling 200-mesh amorphous silicon dioxide and calcium carbonate in a mass ratio of 1:0.05 to obtain a mixture, and heat-treating the mixture at 850° C. for 12 h in a nitrogen atmosphere to obtain modified silicon dioxide;

[0069] (2) At 0° C., 0.4 g of the modified silicon dioxide obtained in step (1) was dispersed in 20 ml of a 1 M phosphoric acid solution, and then 0.4 g of aniline monomer was added and mixed to obtain a solution A;

[0070] (3) Re-take 20 ml of 1 M phosphoric acid solution, add oxidant ammonium persulfate thereto, the molar ratio of ammonium persulfate to aniline monomer added in step (2) is 1:1, stir evenly until colorless and transparent, obtain solution B, add solution B to solution A obtained in step (2), and carry out in-situ polymerization for 6 hours; the polymerization reaction of aniline is a strongly exothermic reaction, first prepare solution B of oxidant ammonium persulfate, and then slowly add it dropwise to solution A, which effectively avoids sudden change in reaction temperature and makes the reaction more complete.

[0071] (4) The product obtained by the in-situ polymerization reaction in step (3) is filtered, washed, and dried, and then sent into a tubular furnace. The temperature is increased to 900° C. at a heating rate of 5° C. / min under a protective nitrogen atmosphere and calcined for 3 h. After natural cooling, the product is ground and pulverized to obtain a nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material.

[0072] Example 5

[0073] A method for preparing a nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material comprises the following steps:

[0074] (1) ball-milling 200-mesh amorphous silicon dioxide and sodium carbonate in a mass ratio of 1:0.05 to obtain a mixture, and heat-treating the mixture at 850° C. for 12 h in a nitrogen atmosphere to obtain modified silicon dioxide;

[0075] (2) At 0° C., 0.4 g of the modified silicon dioxide obtained in step (1) was dispersed in 20 ml of a 1 M phosphoric acid solution, and then 0.4 g of aniline monomer was added and mixed to obtain a solution A;

[0076] (3) Re-take 20 ml of 1 M phosphoric acid solution, add oxidant ammonium persulfate thereto, the molar ratio of ammonium persulfate to aniline monomer added in step (2) is 2:1, stir evenly until colorless and transparent, obtain solution B, add solution B to solution A obtained in step (2), and carry out in-situ polymerization for 6 hours; the polymerization reaction of aniline is a strongly exothermic reaction, first prepare solution B of oxidant ammonium persulfate, and then slowly add it dropwise to solution A, which effectively avoids sudden change of reaction temperature and makes the reaction more complete.

[0077] (4) The product obtained by the in-situ polymerization reaction in step (3) is filtered, washed, and dried, and then sent into a tubular furnace. The temperature is increased to 900° C. at a heating rate of 5° C. / min under a protective nitrogen atmosphere and calcined for 3 h. After natural cooling, the product is ground and pulverized to obtain a nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material.

[0078] Performance Testing

[0079] The nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material prepared in Example 1-3 is used to prepare a negative electrode sheet and a battery, and the method is as follows:

[0080] Negative electrode sheet: The nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material prepared in Example 1-3: the conductive agent: the binder is dissolved in a solvent in a mass ratio of (70-90): (5-20): (5-10) and mixed evenly, then coated on a copper foil current collector and vacuum dried to obtain a negative electrode sheet; Battery: The prepared negative electrode sheet, positive electrode sheet, electrolyte, diaphragm and casing are assembled into a lithium-ion battery using conventional production processes.

[0081] The prepared negative electrode sheet and battery were subjected to performance tests as follows: Button capacity and first coulomb efficiency: The prepared negative electrode sheet was subjected to a button battery test, and the button battery assembly method was as follows: the negative electrode material, the conductive agent and the binder were dissolved in a solvent in a mass percentage of 90:5:5 and mixed, the solid content was controlled at 50%, and the mixture was coated on a copper foil current collector, and vacuum dried to obtain a negative electrode sheet; a metal lithium sheet, 1 mol / L EC+DMC+EMC (v / v=1:1:1)+5% FEC electrolyte, and Celgard 2400 separator were used for the electrode to assemble into a button battery of model LIR2016.

[0082] Cycling performance: The charge and discharge test of the button cell was conducted on a Neware battery test system. At room temperature, the cell was first activated at 0.1C (1C = 500mAh / g) for two cycles, followed by 1C constant current charge and discharge. The charge and discharge voltage was limited to 0.005-2.0V.

[0083] Rate performance: The charge and discharge test of the button cell was conducted on a Neware battery test system at room temperature to test the capacity ratio under 0.1C constant current charging condition and under 1C constant current charging condition.

[0084] Example 1 The first charge-discharge curve of the nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material is as follows: Figure 5 As shown, it can be observed that the reversible capacity of the nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material prepared in Example 1 is 942.3 mAh / g, and the first coulombic efficiency of the material is 75.5%, that is, the nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material prepared in Example 1 has a higher capacity and also has a higher first coulombic efficiency.

[0085] Example 1 The cycle performance of the nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material is shown in the figure Figure 6 As shown in the figure, the rate performance diagram is as follows Figure 7 shown; from Figure 6 and Figure 7 It can be seen that the capacity retention rate of the nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material prepared in Example 1 after 100 cycles at a current density of 1C is as high as 82.4%, indicating that the phosphoric acid-doped aniline coating effect is better. In addition to the cycle stability, in terms of rate performance, the material also shows a more stable and higher discharge specific capacity.

[0086] Example 2 shows the cycle performance of the nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material. Figure 8 As shown, the capacity retention rate after 100 cycles at a current density of 1C is 76%, proving that the phosphoric acid-doped aniline layer can improve the cycling stability of the battery material.

[0087] Example 3 shows the cycle performance of the nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material. Fig. 9 As shown, the capacity retention rate after 100 cycles at a current density of 1C is 72%, proving that the phosphoric acid-doped aniline layer can improve the cycling stability of the battery material.

[0088] Example 4 The first charge-discharge curve of the nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material is as follows: Fig.10 As shown, it can be observed that the reversible capacity of the nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material prepared in Example 4 is 587.5 mAh / g, and the first coulombic efficiency of the material is 76%. Compared with Example 1, the first coulombic efficiency is 0.5% higher, but the reversible capacity is 354.8 mAh / g lower, which can be judged that the effect of modifying silicon oxide with calcium carbonate is not as good as that of sodium carbonate.

[0089] Example 4 shows the cycle performance of the nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material. Fig.11 As shown, the capacity retention rate after 100 cycles at a current density of 1C is 81.5%. Although the prepared material has good cycle performance, the specific capacity is lower than that of Example 1.

[0090] Example 5 shows the cycle performance of the nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material. Fig.12 As shown, the capacity retention rate after 100 cycles at a current density of 1C is 75%. The amount of ammonium persulfate added as the oxidant in Example 5 is twice that of the aniline monomer. The addition of excessive oxidant will increase the polymerization amount of aniline and the overall carbon coating amount, resulting in a lower specific capacity than that in Example 1.

[0091] In summary, adding too much aniline monomer in the preparation method will lead to a larger overall carbon coating amount and reduce the cycle stability; adding too much sodium carbonate will consume a part of the active silicon oxide and reduce the specific capacity; at the same time, it can be seen that the effect of adding metal compounds to modify silicon oxide with sodium carbonate is better than that with calcium carbonate; the molar ratio of ammonium persulfate to aniline monomer is 1:1, which is better. It can be seen that the nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material obtained by the preparation method of Example 1 has better performance.

[0092] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material, It is characterized in that The following steps are involved: (1) ball-milling silicon dioxide and a metal compound to obtain a mixture, and subjecting the mixture to a heat treatment reaction under a protective atmosphere to obtain modified silicon dioxide; The metal compound is an alkali metal compound and / or an alkaline earth metal compound; The metal compound is one or more of sodium carbonate, lithium carbonate, potassium carbonate, calcium carbonate, sodium hydroxide, potassium hydroxide, lithium hydroxide, aluminum oxide, magnesium oxide, and sodium citrate, and the mass ratio of silicon oxide to the metal compound is 1:0.01-0.8; (2) dispersing the modified silicon dioxide obtained in step (1) in a phosphorus source solution at low temperature, and then adding a nitrogen-containing carbon source, and mixing to obtain a solution A; The nitrogen-containing carbon source is aniline monomer and / or pyrrole monomer, and the amount of the nitrogen-containing carbon source added is 1-10 times the amount of the modified silicon oxide added; (3) taking a new phosphorus source solution, adding an oxidant thereto, stirring evenly to obtain a solution B, and adding the solution B to the solution A obtained in step (2) to carry out an in-situ polymerization reaction; The oxidants are ammonium persulfate, potassium persulfate, H 2 O 2 , CuCl 2 A method in which the molar ratio of the oxidant to the nitrogen-containing carbon source in step (2) is 1:1-5; (4) The product obtained by the in-situ polymerization reaction in step (3) is washed and dried, and then subjected to a heat treatment reaction under a protective atmosphere, and then ground and pulverized to obtain a nitrogen-phosphorus co-doped carbon-coated modified silicon oxide negative electrode material.

2. The preparation method according to claim 1, It is characterized in that The reaction temperature of the heat treatment reaction in step (1) is 750-900° C., and the reaction time is 1-24 h.

3. The preparation method according to claim 1, It is characterized in that In step (2), the low temperature is 0-5°C.

4. The preparation method according to claim 1, It is characterized in that In step (2) and step (3), the phosphorus source solutions are one or more of phosphoric acid, phytic acid, hypophosphorous acid, and phosphorous acid, and the concentration of the phosphorus source solution is 0.5M-5M.

5. The preparation method according to claim 1, It is characterized in that The reaction time of the in-situ polymerization reaction in step (3) is 3-24h.

6. The preparation method according to claim 1, It is characterized in that The reaction temperature of the heat treatment reaction in step (4) is 750-900° C., and the reaction time is 1-10 h.

7. A nitrogen and phosphorus co-doped carbon-coated modified silicon oxide negative electrode material prepared by the preparation method according to any one of claims 1 to 6.