A process for preparing building materials products by membrane separation coupled mineralization technology and its application
Through membrane separation and coupling mineralization technology, low-concentration carbon dioxide reacts with solid waste to prepare building materials products, solving the problems of low-concentration carbon dioxide capture and solid waste disposal, and achieving efficient carbon utilization and energy consumption reduction.
Patent Information
- Application Number
- CN202211115191.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-14
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-09-14
AI Technical Summary
When collecting low-concentration carbon dioxide gases, it is difficult to effectively utilize and reduce the energy consumption of the carbon capture process, and industrial applications are limited by the demand for high-concentration carbon dioxide.
Using membrane separation and coupling mineralization technology, the low-concentration carbon dioxide in flue gas is captured and reacted with solid waste to prepare building materials, use high-concentration carbon dioxide-containing gas with a certain humidity to carry out mineralization reaction, and recycle mineralization The water vapor and heat generated by the reaction.
It has achieved efficient utilization of low-concentration carbon dioxide, reduced the cost of solid waste disposal and energy consumption of carbon capture process, and prepared building materials with excellent performance, solving the company's solid waste disposal and carbon emission problems.
Smart Images

Figure CN115838259B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of building materials, and in particular to a process for preparing building materials by using membrane separation coupled mineralization technology and its application. Background Art
[0002] CO2 capture, utilization and storage (CCUS) is an important means to reduce the concentration of CO2 in the atmosphere and thus inhibit the greenhouse effect. my country has developed carbon emission rights to control carbon emissions in response to corporate carbon emissions. At the same time, the CO2 concentration of most large emission sources is less than 15%. For example, the flue gas emitted by coal-fired thermal power plants is mainly composed of about 5% to 20% water vapor and 10% to 15% carbon dioxide. Therefore, the capture and utilization technology for low-concentration carbon dioxide gas is extremely necessary.
[0003] However, many current utilization technologies have high requirements for the concentration of carbon dioxide, such as carbon dioxide oil recovery, carbon dioxide geological storage, and carbon dioxide chemical utilization. However, this has also led to the current carbon capture process targeting high-concentration carbon dioxide; for example, patent CN113603828B proposes a carbon dioxide capture agent and its preparation method, which is carried out at 40-80°C and desorbed at a high temperature of 110-130°C, with an average purity of more than 90%; patent application document CN111298604A proposes a system and method for capturing carbon dioxide in flue gas, which can optimize the capture of carbon dioxide in flue gas and achieve a carbon dioxide capture rate of ≥90% and a carbon dioxide concentration of >99%. However, patent application document CN 112516758A proposes a secondary membrane separation system and method for capturing carbon dioxide in flue gas, which can enrich carbon dioxide to about 70%, and the captured gas contains a certain amount of water vapor, which makes it impossible to use it for the various utilizations mentioned above, so its industrial application scenario is relatively low.
[0004] Therefore, in order to solve the above problems, the present application provides a process for preparing building materials products by using membrane separation coupled mineralization technology, which can fully utilize the high-concentration carbon dioxide gas directly captured after membrane separation and greatly improve the production efficiency of building materials products. Summary of the invention
[0005] In order to solve the above problems, the first aspect of the present invention provides a process for preparing building materials products by membrane separation coupled with mineralization technology, and the process steps include the following steps:
[0006] S1. The flue gas is separated and captured by membrane to obtain high-concentration carbon dioxide gas with a certain humidity;
[0007] S2. The carbon dioxide-containing gas obtained by membrane separation is used to mineralize the green body made of solid waste to prepare building materials.
[0008] As a preferred solution, step S1 includes the following steps:
[0009] S11, sending the flue gas to the dust removal, desulfurization and denitrification device for pretreatment to remove harmful gases and impurities;
[0010] S12, introducing the pretreated flue gas into the first buffer tank, and then entering the first-stage membrane separator to separate and capture carbon dioxide after being compressed by the first compressor;
[0011] S13, the captured gas from the first-stage membrane separator is introduced into the second buffer tank, and then compressed by the second compressor and introduced into the humidification tank. After humidification in the humidification tank, it enters the second-stage membrane separator to capture and separate carbon dioxide, thereby obtaining a carbon dioxide-containing gas with a high concentration and a certain humidity.
[0012] As a preferred solution, the flue gas is any one of power plant flue gas, coal-fired power plant flue gas, lime kiln flue gas, steel plant flue gas, chemical plant flue gas, cement plant flue gas, and carbon capture flue gas.
[0013] As a preferred solution, in the high-concentration carbon dioxide-containing gas with a certain humidity, the volume percentage of carbon dioxide is 60-80%, and the volume percentage of water vapor is 5-30%.
[0014] As a preferred solution, the volume percentage of water vapor in the high-concentration carbon dioxide-containing gas with a certain humidity is 10-20%.
[0015] As a preferred solution, step S2 includes the following steps:
[0016] S21, mixing solid waste, an additive and water to obtain a mixture, and placing the mixture into a mold to form a green body;
[0017] S22, the green body is sent into a closed reactor, and the high-concentration and humidity carbon dioxide-containing gas obtained in step S1 is introduced, so that the gas and the green body are in direct contact with each other to cause a mineralization reaction, thereby obtaining a building material product.
[0018] As a preferred solution, the molding method in step S21 is compression molding, and the molding pressure is 3 to 30 MPa, preferably, the molding pressure is 5 to 20 MPa.
[0019] As a preferred solution, the gas discharged during the mineralization reaction or the gas remaining in the reactor after the mineralization reaction is completed is introduced into a dust removal chamber for dust removal and recovery of heat and water vapor. The gas with a certain humidity passing through the dust removal chamber is sent to the first buffer tank for recycling.
[0020] As a preferred solution, the temperature of the gas after being treated in the dust removal chamber is controlled at 20-60°C, the temperature of the gas entering the first-stage membrane separator is controlled at 20-60°C, and the temperature of the gas entering the second-stage membrane separator is controlled at 20-60°C.
[0021] As a preferred solution, the temperature of the first-stage membrane separator and the second-stage membrane separator is 1-10°C higher than the temperature of the flue gas about to enter the first-stage membrane separator and the second-stage membrane separator. The higher temperature of the first-stage membrane separator and the second-stage membrane separator can prevent the condensation of water vapor in the flue gas.
[0022] As a preferred solution, the separation pressure of the first-stage membrane separator is 3.5 to 5.9 bar; the separation pressure of the second-stage membrane separator is 3.7 to 5.9 bar.
[0023] As a preferred solution, the reaction pressure of the mineralization reaction is 0.1-1 MPa, and the reaction time is 1-24 hours.
[0024] As a preferred solution, the reaction pressure of the mineralization reaction is 0.4-0.8 MPa, and the reaction time is 2-12 hours.
[0025] As a preferred solution, the mineralizable solid waste in the solid waste accounts for 5-40% by mass of the total solid waste; the additive accounts for 0.1-5% by mass of the total solid waste; and the water accounts for 5-30% by mass of the solid waste.
[0026] As a preferred solution, the mass percentage of the auxiliary agent to the total amount of solid waste is 0.5-3%, and the mass percentage of the water to the solid waste is 8-20%.
[0027] As a preferred solution, the solid waste includes calcareous solid waste and siliceous and aluminum-silicon solid waste.
[0028] As a preferred solution, the calcareous solid waste is one or more of carbide slag, waste lime, waste cement, steel slag, slag, magnesium slag, and red mud.
[0029] As a preferred solution, the silicoaluminous solid waste is selected from one or more of fly ash, phosphorus desulfurization gypsum, slag, building waste, yellow phosphorus slag, fly ash, smelting slag, and red mud.
[0030] As a preferred solution, the auxiliary agent is at least one of diatomaceous earth, expanded perlite, red jade, zeolite, and sandstone.
[0031] As a preferred solution, the ventilation speed of the high-concentration and humidity-containing carbon dioxide gas is 40 to 200 m / s. 3 / min.
[0032] As a preferred solution, the ventilation speed of the high-concentration and humidity-containing carbon dioxide gas is 60 to 120 3 / min, and the required gas needs to be introduced within 30 minutes before the reaction.
[0033] The second aspect of the present invention provides an application of the above-mentioned membrane separation coupled mineralization technology to prepare building materials products, including the application of the process in carbon capture synergistic mineralization reaction to prepare building materials products.
[0034] Beneficial effects:
[0035] 1. The present invention proposes a process for preparing building materials products by coupling membrane separation with mineralization technology. By coupling membrane decomposition technology with mineralization technology, it provides a technical method for synergistic mineralization treatment of bulk solid waste for low-concentration carbon dioxide emission enterprises, greatly reducing the cost of solid waste disposal, and is conducive to the promotion and application of this process in low-concentration, high-carbon emission and high solid waste output enterprises.
[0036] 2. The present invention proposes a process for preparing building materials products by using membrane separation coupled with mineralization technology. The process utilizes the high-concentration and humidity carbon dioxide-containing gas captured by membrane separation. The water vapor contained in the gas can maintain the humidity of the mineralization reaction system to improve the mineralization efficiency. On the other hand, the water vapor and heat generated by the mineralization reaction are recycled to membrane separation to achieve the promotion of membrane separation and mineralization technology. It not only absorbs the waste carbon dioxide in the production of the enterprise, but also reduces the energy consumption of the carbon capture process, making full use of solid waste to prepare building materials products with excellent performance.
[0037] 3. The present invention proposes a process for preparing building materials products by using membrane separation coupled mineralization technology. The process can utilize only 70-80% volume concentration of carbon dioxide-containing gas after membrane separation capture to achieve the preparation of mineralized and hydrated building materials products. This is different from the existing mineralization process for preparing building materials, which requires ultra-high concentration of carbon dioxide-containing gas of about 99%. It greatly reduces the cost of industrial production and effectively realizes the efficient resource utilization of solid waste in enterprises. The products prepared by the process have excellent performance and good carbon fixation performance, which not only solves the solid waste disposal and carbon emission problems of enterprises. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 Schematic diagram of the process flow for preparing building materials products using membrane separation coupled mineralization technology provided in this application. DETAILED DESCRIPTION
[0039] In the examples of the present application, the solid waste used is a mixture of steel slag and recycled aggregate from a steel plant. The moisture content of the steel slag is 2.6wt%, and the chemical composition is shown in the following table:
[0040] Table 1 Main element composition of steel slag
[0041] Elemental composition CaO <![CDATA[Fe2O3]]> <![CDATA[SiO2]]> MgO <![CDATA[Al2O3]]> MnO <![CDATA[TiO2]]> <![CDATA[P2O5]]> LOSS Content wt% 36.79 22.31 15.21 6.37 4.52 2.76 2.13 1.44 8.47
[0042] The chemical composition of recycled aggregate is shown in the following table:
[0043] Table 2 Main element composition of recycled aggregate
[0044] Elemental composition <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[CO2]]> CaO <![CDATA[Fe2O3]]> <![CDATA[K2O]]> MgO <![CDATA[Na2O]]> LOSS Content wt% 47.2 16.5 17.2 8.13 3.55 1.63 1.37 0.81 3.61
[0045] The flue gas is from a steel plant, and its chemical composition is shown in the following table:
[0046] Table 3 Gas composition (volume fraction) of flue gas from a steel plant
[0047] Gas composition <![CDATA[CO2]]> <![CDATA[N2]]> <![CDATA[H2O (vapor)]]> CO LOSS content% 15.5 63.3 10.3 13.2 0.9
[0048] The process for preparing building materials products using membrane separation coupled mineralization technology used in each embodiment of the present application includes the following steps:
[0049] S1. The flue gas is separated and captured by membrane to obtain high-concentration carbon dioxide gas with a certain humidity;
[0050] S11, send the flue gas to the dust removal, desulfurization and denitrification device for pretreatment to remove NO x 、SO x and harmful gases and impurities such as dust;
[0051] S12, introducing the pretreated flue gas into the first buffer tank, step S22, after the mineralization reaction is completed, the remaining gas in the reactor is introduced into the dust removal chamber for dust removal, and the gas with a certain humidity after passing through the dust removal chamber is also sent to the first buffer tank, the pretreated flue gas and the dust-removed flue gas are mixed, and then compressed by the first compressor. The temperature of the mixed flue gas is about 20-60°C and enters the first-stage membrane separator to separate and capture carbon dioxide. The separation pressure of the first-stage membrane separator is 3.5-5.9 bar;
[0052] S13, the captured gas of the first-stage membrane separator is introduced into the second buffer tank, and then compressed by the second compressor and introduced into the humidification tank. After humidification in the humidification tank, the flue gas temperature is about 20-60°C, and enters the second-stage membrane separator to capture and separate carbon dioxide, that is, a high-concentration carbon dioxide-containing gas with a certain humidity is obtained. The separation pressure of the second-stage membrane separator is 3.7-5.9 bar;
[0053] S2. Using the carbon dioxide-containing gas obtained by membrane separation and capture to mineralize the green body made of solid waste to prepare building materials;
[0054] S21, mixing solid waste, additives and water to obtain a mixture, and placing the mixture into a mold and pressing it at a molding pressure of 3-30 MPa to obtain a green body;
[0055] S22, the green body is sent into a closed reactor, and the high-concentration and humidity carbon dioxide-containing gas obtained in step S1 is introduced, so that the gas and the green body are in direct contact with each other to cause a mineralization reaction, thereby obtaining a building material product.
[0056] Performance Testing Methods
[0057] Weight gain rate: The carbon fixation rate in this experiment is expressed as the weight gain rate of the test block.
[0058] The mass change before and after CO2 curing is determined by mass weighing method, and the weight gain rate is calculated as follows:
[0059]
[0060] Where ω is the apparent weight gain rate,
[0061] m0 is the dry mass after CO2 pressing,
[0062] m1 is the mass of the specimen after CO2 curing (mass after drying).
[0063] The specific steps are as follows:
[0064] 1. Determine the moisture content w1 of the raw materials after digestion, weigh the mass of the brick after pressing, and calculate the corresponding dry basis mass m0 in the test block based on the moisture content after digestion
[0065] 2. After the test block is mineralized, dry the test block to make it constant weight and then measure its dry basis mass as m1.
[0066] 3. Use the above formula to calculate the corresponding test block weight gain rate
[0067] Note: PTY-B5000 electronic balance is used for measurement. Range: 5kg. Linear error: ±0.04g. Five samples are tested for each comparative example. The measured values are the average value.
[0068] Compressive strength test: The compressive strength is measured in accordance with GBT4111-2013 "Test methods for concrete blocks and bricks". The strength is measured after the test pieces are naturally air-dried for 24 hours.
[0069] 1. Test steps
[0070] 1. Measure the length and width of each specimen’s connection surface or pressure surface twice, and take their average values, accurate to 1mm.
[0071] 2. Place 10 test pieces flat on the center of the pressure plate and apply load perpendicular to the pressure surface. The load should be even and stable without any impact or vibration.
[0072] The loading speed is (5±0.5) kN / s until the specimen is destroyed, and the maximum failure load F (in N) is recorded.
[0073] 2. Calculation of test results
[0074] 1. Calculate the compressive strength of 10 bricks according to the following formula, accurate to 0.1MPa.
[0075]
[0076] Where f mc —compressive strength (MPa);
[0077] F—maximum failure load (N);
[0078] L—length of the pressure surface (connection surface) (mm);
[0079] B—Width of the pressure surface (connection surface) (mm).
[0080] Calculate the average compressive strength of three to five test blocks. If the difference between the measured values and their average value is not greater than 15%, use the average value as the compressive strength; if the difference between a certain value and the average value is greater than 15%, this value should be discarded and the average value should be calculated with the remaining values. Five samples are tested for each embodiment and comparative example, and the average value of the measured values is calculated.
[0081] Example 1
[0082] The volume percentage composition of the high-concentration and humidity-containing carbon dioxide gas obtained by membrane separation capture is as follows:
[0083] Table 4 Gas composition (volume fraction) of high concentration and humidity carbon dioxide-containing gas
[0084] Gas composition <![CDATA[CO2]]> <![CDATA[H2O]]> <![CDATA[N2]]> LOSS content% 74.5 18.9 6.2 0.4
[0085] Preparation of green bricks: 60 parts of steel slag, 115.5 parts of recycled aggregate and 24.4 parts of water are mixed evenly to obtain a mixture, and the mixture is placed in a mold and pressed at a molding pressure of 10 MPa to obtain a green brick. The brick shape is 200 mm*95 mm*53 mm.
[0086] Mineralization reaction: The green body is sent into the reactor, and the captured carbon dioxide-containing gas is introduced into the reactor for mineralization reaction. The reaction pressure is 0.6MPa and the reaction time is 6 hours. The initial reaction temperature is 25℃ and the ventilation rate is 73m / s. 3 / min, the CO2 concentration in the carbon dioxide-containing gas is 74.5%, and the water vapor concentration is 18.9%.
[0087] In this embodiment, the process flow diagram of the process flow is as follows Figure 1 shown.
[0088] The weight gain rate of the building material product prepared in this embodiment is 7.74%, and the compressive strength is 22.52 MPa.
[0089] Example 2
[0090] The specific implementation of this embodiment is the same as that of Embodiment 1, except that the carbon dioxide-containing gas used in this embodiment is a formulated gas (excluding the influence of carbon dioxide concentration on the experiment, and only investigating the influence of water content on the experiment), and the gas composition (volume fraction) is CO2 74.5%, H2O 5%, and N2 20.5%.
[0091] The weight gain rate of the obtained product is 4.17% and the compressive strength is 11.26 MPa.
[0092] Example 3
[0093] The specific implementation of this embodiment is the same as that of Embodiment 2, except that: the carbon dioxide-containing gas used in this embodiment is a formulated gas (excluding the influence of carbon dioxide concentration on the experiment, and only investigating the influence of water content on the experiment), and the gas composition (volume fraction) is CO2 74.5%, H2O 10%, and N2 15.5%.
[0094] The weight gain rate of the obtained product is 5.53%, and the compressive strength is 17.26MPa.
[0095] Example 4
[0096] The specific implementation of this embodiment is the same as that of Embodiment 3, except that the carbon dioxide-containing gas used in this embodiment is a formulated gas (excluding the influence of carbon dioxide concentration on the experiment, and only investigating the influence of water content on the experiment), and the gas composition (volume fraction) is CO2 74.5%, H2O 20%, and N2 5.5%.
[0097] The weight gain rate of the obtained product is 5.72%, and the compressive strength is 16.24 MPa.
[0098] Example 5
[0099] The specific implementation of this embodiment is the same as that of Example 4, except that: the carbon dioxide-containing gas used in this embodiment is a formulated gas (excluding the influence of carbon dioxide concentration on the experiment, and only investigating the influence of water content on the experiment), and the gas composition (volume fraction) is CO2 74.5%, H2O 25%, and N2 0.5%.
[0100] The weight gain rate of the obtained product is 3.21%, and the compressive strength is 10.16MPa.
[0101] Example 6
[0102] The specific implementation of this embodiment is the same as that of Embodiment 1, except that the mixture (by weight) contains 60 parts of steel slag, 131.5 parts of recycled aggregate, and 8.4 parts of water.
[0103] The weight gain rate of the obtained product is 2.73%, and the compressive strength is 7.45MPa.
[0104] Example 7
[0105] The specific implementation of this embodiment is the same as that of Embodiment 1, except that the mixture (by weight) contains 60 parts of steel slag, 125.5 parts of recycled aggregate, and 14.4 parts of water.
[0106] The weight gain rate of the obtained product is 5.64%, and the compressive strength is 16.45 MPa.
[0107] Example 8
[0108] The specific implementation of this embodiment is the same as that of Embodiment 1, except that: the mixture (by weight) contains 60 parts of steel slag, 101.5 parts of recycled aggregate, and 38.4 parts of water.
[0109] The weight gain rate of the obtained product is 5.31%, and the compressive strength is 15.79 MPa.
[0110] Example 9
[0111] The specific implementation of this embodiment is the same as that of Embodiment 1, except that: the mixture (by weight) contains 60 parts of steel slag, 91.5 parts of recycled aggregate, and 48.4 parts of water.
[0112] The weight gain rate of the obtained product is 2.33%, and the compressive strength is 7.26MPa.
[0113] Example 10
[0114] The specific implementation of this embodiment is the same as that of Embodiment 1, except that the green body molding pressure is 3 MPa.
[0115] The weight gain rate of the obtained product is 7.89% and the compressive strength is 10.26 MPa.
[0116] Embodiment 11
[0117] The specific implementation of this embodiment is the same as that of embodiment 1, except that: the green body molding pressure is 5 MPa
[0118] The weight gain rate of the obtained product is 7.64% and the compressive strength is 16.31 MPa.
[0119] Example 12
[0120] The specific implementation of this embodiment is the same as that of embodiment 1, except that: the green body molding pressure is 20 MPa
[0121] The weight gain rate of the obtained product is 5.23%, and the compressive strength is 15.26 MPa.
[0122] Example 13
[0123] The specific implementation of this embodiment is the same as that of embodiment 1, except that: the green body molding pressure is 30 MPa
[0124] The weight gain rate of the obtained product is 2.13%, and the compressive strength is 7.17 MPa.
[0125] Embodiment 14
[0126] The specific implementation of this embodiment is the same as that of Embodiment 1, except that: the mixture contains 60 parts of steel slag, 114.5 parts of recycled aggregate, 1 part of diatomaceous earth, and 24.4 parts of water.
[0127] The weight gain rate of the obtained product is 8.12%, and the compressive strength is 24.52MPa.
[0128] Embodiment 15
[0129] The specific implementation of this embodiment is the same as that of Embodiment 1, except that: the mixture contains 60 parts of steel slag, 113.5 parts of recycled aggregate, 2 parts of diatomaceous earth, and 24.4 parts of water.
[0130] The weight gain rate of the obtained product is 9.13%, and the compressive strength is 26.54 MPa.
[0131] Example 16
[0132] The specific implementation of this embodiment is the same as that of Embodiment 1, except that: the mixture contains 60 parts of steel slag, 109.5 parts of recycled aggregate, 6 parts of diatomaceous earth, and 24.4 parts of water.
[0133] The weight gain rate of the obtained product is 8.71%, and the compressive strength is 25.71 MPa.
[0134] Embodiment 17
[0135] The specific implementation of this embodiment is the same as that of Embodiment 1, except that: the mixture contains 60 parts of steel slag, 105.5 parts of recycled aggregate, 10 parts of diatomaceous earth, and 24.4 parts of water.
[0136] The weight gain rate of the obtained product is 6.32%, and the compressive strength is 17.36MPa.
[0137] Embodiment 18
[0138] The specific implementation of this embodiment is the same as that of Embodiment 1, except that: the mixture contains 60 parts of steel slag, 113.5 parts of recycled aggregate, 2 parts of expanded perlite, and 24.4 parts of water.
[0139] The weight gain rate of the obtained product is 9.32%, and the compressive strength is 27.32 MPa.
[0140] Comparing Examples 1-5, it can be seen that Examples 1-5 use carbon dioxide-containing gas with a water vapor content of 5-25%, and the weight gain rate of the prepared building materials is 3.21-7.74%, and the compressive strength reaches 10.16-22.52MPa, which has a good carbon fixation effect and a high compressive strength. Among them, the weight gain rate and compressive strength of the building materials prepared by Examples 1 and 3-4 are better. This is because the carbon dioxide-containing gas contains an appropriate amount of water vapor, which makes the humidity in the environment more suitable, and the moisture in the block is retained inside the block. The carbon dioxide can dissolve in the moisture in the block and then react with the mineralizable substance, thereby obtaining a higher carbon fixation effect and compressive strength. In Example 2, because the water vapor content in the carbon dioxide-containing gas is only 5%, the water vapor content in the environment is too low, causing the moisture in the block to evaporate into the environment, resulting in a low degree of mineralization reaction and low compressive strength. In Example 5, the water vapor content in the carbon dioxide-containing gas is as high as 25%. The excessive water vapor content makes the system environment humidity too high, and the water vapor blocks the pores of the green body, which is not conducive to the entry of carbon dioxide into the green body, affecting the degree of mineralization reaction, the carbon fixation effect is poor, and the compressive strength is low. Therefore, it is preferred that the volume percentage of water vapor in the carbon dioxide-containing gas obtained by membrane separation capture is 10-20%.
[0141] Comparing Example 1 with Examples 6-9, it can be seen that the mass percentage of water in the total amount of solid waste (steel slag and recycled aggregate) in these examples is 13.9%, 4.4%, 7.8%, 23.8% and 31.9% respectively, and the weight gain rate of the prepared building materials is 2.33-7.74%, and the compressive strength reaches 7.26-22.52MPa, which has good carbon fixation effect and high compressive strength. Among them, the carbon fixation effect and compressive strength of the building materials prepared in Example 1 and Examples 7-8 are better, because the appropriate water content inside the block can ensure that the system has the appropriate moisture content required for mineralization, and at the same time, the channel for carbon dioxide diffusion inside the blank will not be blocked due to excessively high moisture content, thereby having a higher weight gain rate and compressive strength. In Example 6, when the mass percentage of water in the total amount of solid waste was only 4.4%, the weight gain rate of the prepared building material product was only 2.73%, and the compressive strength was only 7.45MPa. This is because the water content of the system is too low, but the mineralization reaction requires the participation of water. Too little water makes the degree of mineralization reaction low, resulting in low carbon fixation effect and compressive strength of the building material product. In Example 9, when the mass percentage of water in the total amount of solid waste reached 31.9%, the weight gain rate of the prepared building material product was only 2.33%, and the compressive strength was only 7.26MPa. This is because the water content of the system is too high, causing the water to block the diffusion channel of carbon dioxide and reduce the degree of mineralization reaction, thereby affecting the weight gain rate and compressive strength. Therefore, preferably, the mass percentage of water in solid waste is 8-20%.
[0142] Comparing Example 1 with Examples 10-13, it can be seen that the pressures for green compacting in these examples are 10MPa, 3MPa, 5MPa, 20MPa and 30MPa, respectively, and the weight gain rate of the prepared building materials is 2.13-7.74%, and the compressive strength is 7.17-22.52MPa, which has a good carbon fixation effect and a high compressive strength. Among them, the carbon fixation effect and compressive strength of the building materials prepared in Examples 1 and 11-12 are better, because the appropriate molding pressure can, on the one hand, have a suitable binding force between the components in the green body, and at the same time retain a certain carbon dioxide diffusion channel. During the mineralization process, carbon dioxide diffuses into the green body for mineralization reaction, and the formed mineralized product makes the ten internal materials fit tightly, which on the one hand ensures the carbon fixation effect, and on the other hand helps to increase the strength of the green body. In Example 10, the molding pressure is only 3MPa, and the lower molding pressure, the green body has more pores, and the carbon dioxide can fully react with the mineralizable substances inside the green body, so that the degree of mineralization reaction is higher, but because the components cannot be tightly combined, the compressive strength is still low. In Example 13, the molding pressure is as high as 30 MPa, and the weight gain rate and compressive strength of the prepared building materials are also relatively low. This is because the molding pressure is too high during pressing, the interior of the green body is too dense, the diffusion of carbon dioxide is hindered, and it is basically unable to enter the interior of the green body, resulting in a low degree of mineralization reaction, and low carbon fixation effect and compressive strength.
[0143] Comparing Example 1 with Examples 14-17, it can be seen that the weight gain rate of the building material products prepared in each embodiment reaches 6.32-9.13%, and the compressive strength reaches 17.13-26.54MPa, and the effects are all relatively good. Among them, the weight gain rate (carbon fixation effect) and compressive strength of Examples 14-16 are better than those of Example 1. This is probably because diatomaceous earth can adjust the moisture content inside the body to achieve a suitable environmental humidity, which is conducive to the mineralization reaction. The mineralization degree is high, and the weight gain rate and compressive strength of the product are both high. When the diatomaceous earth addition amount reaches 10 parts in Example 17, the weight gain rate and compressive strength of the prepared building material products are significantly lower than those in Example 1. This may be due to the fact that the diatomaceous earth dosage is too high, the diatomaceous earth adjusts the water imbalance, and the environment moisture content cannot be controlled to be optimal. At the same time, because the diatomaceous earth is too loose, it is easy to become microcracks inside the product, and then the mineralization degree of the product decreases, and the compressive strength of the product decreases. Therefore, when the mass percentage of the additive to the total amount of solid waste is preferably 0.5-3%, a better product weight gain rate and compressive strength can be obtained.
[0144] By comparing Example 15 and Example 18, it can be seen that when the diatomaceous earth in Example 15 is replaced with an equal weight portion of expanded perlite, the prepared building material product also has a better weight gain rate and compressive strength. This may be because the expanded perlite also has the function of adjusting the humidity of the test block environment. The appropriate dosage enables the test block to maintain the humidity environment required for the mineralization reaction, and the product has high mineralization efficiency, high degree of mineralization, and high compressive strength.
Claims
1. A process for preparing building materials products by membrane separation coupled with mineralization technology, characterized in that: The process steps include the following steps: S1. The flue gas is separated and captured by membrane to obtain high-concentration carbon dioxide gas with a certain humidity; S2. Using membrane separation to capture the carbon dioxide gas-containing mineralized solid waste to make a green body to prepare building materials; The step S2 comprises the following steps: S21, mixing solid waste, an additive and water to obtain a mixture, and placing the mixture into a mold to form a green body; S22, the green body is sent into a closed reactor, and the high-concentration and humidity carbon dioxide-containing gas obtained in step S1 is introduced, so that the gas and the green body are in direct contact with each other to cause a mineralization reaction, thereby obtaining a building material product; The mass percentage of mineralizable solid waste in the solid waste is 5-40% of the total solid waste, and the mass percentage of water in the solid waste is 8-20%; In the high-concentration carbon dioxide-containing gas with a certain humidity, the volume percentage of carbon dioxide is 60-80%, and the volume percentage of water vapor is 10-20%; the auxiliary agent is one or more of diatomaceous earth, expanded perlite, red jade, zeolite, and sandstone; the mass percentage of the auxiliary agent to the total amount of solid waste is 0.1-5%; The molding pressure is 5 to 20 MPa; The solid waste includes calcareous solid waste and silicoaluminous solid waste; the calcareous solid waste is selected from one or more of carbide slag, waste lime, waste cement, steel slag, slag, magnesium slag, and red mud; the silicoaluminous solid waste is selected from one or more of phosphorus desulfurization gypsum, slag, construction waste, yellow phosphorus slag, fly ash, smelting slag, and red mud.
2. The process for preparing building materials products by membrane separation coupled mineralization technology according to claim 1, characterized in that: The step S1 comprises the following steps: S11, sending the flue gas to the dust removal, desulfurization and denitrification device for pretreatment to remove harmful gases and impurities; S12, introducing the pretreated flue gas into the first buffer tank, and then entering the first-stage membrane separator to separate and capture carbon dioxide after being compressed by the first compressor; S13, the captured gas from the first-stage membrane separator is introduced into the second buffer tank, and then compressed by the second compressor and introduced into the humidification tank. After humidification in the humidification tank, it enters the second-stage membrane separator to capture and separate carbon dioxide, thereby obtaining a carbon dioxide-containing gas with a high concentration and a certain humidity.
3. The process for preparing building materials products by membrane separation coupled mineralization technology according to claim 1, characterized in that: After the mineralization reaction is completed, the remaining gas in the reactor is introduced into the dust removal chamber for dust removal, and the gas with a certain humidity passing through the dust removal chamber is sent to the first buffer tank for recycling.
4. The process for preparing building materials products by membrane separation coupled mineralization technology according to claim 3 is characterized in that: The temperature of the gas after being treated in the dust removal chamber is controlled at 20-60°C, the temperature of the gas entering the first-stage membrane separator is controlled at 20-60°C, and the temperature of the gas entering the second-stage membrane separator is controlled at 20-60°C.
5. The process for preparing building materials products by membrane separation coupled mineralization technology according to claim 4, characterized in that: The ventilation speed of the high-concentration and humidity-containing carbon dioxide gas is 40-200 m / s. 3 / min.
6. An application of the process for preparing building materials products by the membrane separation coupled mineralization technology according to any one of claims 1 to 5, characterized in that: This includes the application of this process in the preparation of building materials products through carbon capture and synergistic mineralization reactions.
Citation Information
Patent Citations
System and method for capturing carbon dioxide in flue gas
CN111298604A
Secondary membrane separation system and method for capturing carbon dioxide in flue gas
CN112516758A
A carbon dioxide trap and its preparation method
CN113603828B
Reinforced process for capturing carbon dioxide in flue gas by membrane separation method
CN113491929A
Energy-saving carbon dioxide trapping system and method thereof
CN114904372A