A method for regenerating high-strength negative carbon building materials from Ca-based solid waste and its application

Through the exothermic reaction between Ca-based solid waste and carbon dioxide, the temperature is regulated, and the hydrothermal reaction without external heating sources is achieved, the problems of high energy consumption and carbon emissions in the existing technology are solved, and high-strength and low-carbon building materials are prepared. The efficient resource utilization of solid waste has been achieved.

CN116750985BActive Publication Date: 2024-11-26JIANGSU JICUI FUNCTIONAL MATERIALS RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310050712.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-07-21
Filing Date
2023-02-01
Publication Date
2024-11-26
Estimated Expiration
2043-02-01

AI Technical Summary

Technical Problem

The prior art requires high temperatures during the mineralization reaction, which leads to high energy consumption and difficulty in effectively utilizing solid waste, and there is carbon emission problem with mineralization methods.

Method used

By reacting Ca-based solid waste with carbon dioxide, exothermic reaction is used to regulate the temperature, and hydrothermal reaction without external heating sources is achieved, and high-strength building materials are prepared.

Benefits of technology

It reduces the energy consumption of solid waste treatment, improves the carbon sequestration rate and mechanical strength of building materials, reduces carbon emissions, and realizes efficient resource utilization of solid waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
  • Figure HDA0004291881610000011
    Figure HDA0004291881610000011
Patent Text Reader

Abstract

The present invention relates to the field of building material technology, and in particular to a method for regenerating high-strength negative carbon building materials from Ca-based solid waste and its application. The method for regenerating high-strength negative carbon building materials from Ca-based solid waste is as follows: by controlling the mineralizable calcium component in the reaction raw materials to control the degree of mineralization reaction in the system, the heat released by the mineralization reaction is used to regulate the temperature of the system to achieve the conditions required for the hydrothermal reaction, so that both the mineralization reaction and the hydrothermal reaction can be carried out in the system, thereby obtaining high-strength finished building materials. The present invention effectively realizes the efficient resource utilization of industrial solid waste, and the total carbon emissions of the prepared building materials products are more than 50% lower than those of traditional silicate cement products, which has an important role in promoting the low-carbon development of my country's building materials industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of building materials, and in particular to a method for regenerating high-strength negative carbon building materials using Ca-based solid waste and applications thereof. Background Art

[0002] In recent years, using industrial solid waste as raw materials and making it into building materials through some recycling and processing methods is an effective way to utilize resources. This method can meet the development needs of green environmental protection on the one hand, and meet the goal of solid waste resource utilization on the other hand. It is a feasible route to save resources, protect the environment, eliminate waste, and achieve a "win-win" situation.

[0003] At present, the main technical means for recycling building materials is mineralization. For example, Chinese patent document CN109126412B provides a method for strengthening the mineralization of carbon dioxide from solid waste by using salt-containing wastewater. The solid waste is humidified and then dried, and then the flue gas treated with wastewater is mineralized to effectively capture carbon dioxide and realize the utilization of large amounts of solid waste. However, this prior art requires a temperature of 450-650°C during the mineralization reaction. Chinese patent document CN104987034B provides a method for preparing building bricks by direct carbonization of slag. The solid waste is ball-milled and then mineralized. A temperature of 30-180°C is required during the mineralization reaction. This part of heat increases the carbon emissions of the entire process. The mineralization methods of the current prior art all require a certain amount of heat to be provided to the system, which has the problem of high energy consumption. Summary of the invention

[0004] The present invention provides a method for regenerating high-strength negative carbon building materials using Ca-based solid waste, thereby solving the technical problems of large solid waste emissions, large demand for building materials, high energy consumption in solid waste treatment, and difficulty in resource recycling. By using technical means without the need for external heat sources, Ca-based solid waste is used to fix industrial tail gas source CO2 to prepare high-strength building materials.

[0005] During the actual research process, this applicant found that the reaction between carbon dioxide and mineralizable calcium in solid waste is an exothermic reaction. Utilizing this part of heat can not only meet the temperature required for the mineralization reaction, but also reduce energy consumption. However, there are few studies on the utilization of this part of heat.

[0006] The first aspect of the present invention provides a method for regenerating high-strength negative carbon building materials using Ca (calcium)-based solid waste. The degree of mineralization reaction in the system is controlled by controlling the mineralizable calcium component in the reaction raw materials, and the temperature of the system is regulated by utilizing the heat released by the mineralization reaction to achieve the conditions required for the hydrothermal reaction, so that both mineralization reaction and hydrothermal reaction can be carried out in the system, thereby producing high-strength building materials.

[0007] In some preferred embodiments, the method of regenerating high-strength negative carbon building materials from Ca-based solid waste does not use an external heat source or require additional water vapor.

[0008] In some preferred embodiments, the method for regenerating high-strength negative carbon building materials from Ca-based solid waste comprises the following steps:

[0009] S1. Using Ca-based solid waste for processing to prepare building material prefabricated products;

[0010] S2. Transfer the prefabricated building materials to a reactor, introduce CO2-containing gas to carry out a composite mineralization reaction, and obtain a high-strength negative carbon building material product.

[0011] In some preferred embodiments, the raw materials of the Ca-based solid waste include carbonized materials and auxiliary materials.

[0012] The carbonized material includes, but is not limited to, one or more of carbide slag, fly ash, and white mud.

[0013] Furthermore, the mass fraction of calcium-based components (calcium oxide and / or calcium hydroxide) in the carbonized material is not less than 80%.

[0014] The auxiliary materials include, but are not limited to, one or more of fly ash, bottom ash, red mud, construction waste, waste cement, tailings, and ore raw materials.

[0015] Further preferably, the raw materials of the Ca-based solid waste include carbonized materials and auxiliary materials, and the weight ratio of the carbonized materials to the auxiliary materials is (10-40): (40-80).

[0016] The inventor found in the process of exploration that the preformed product obtained by stirring, powder mixing, digesting and pressing the Ca-based solid waste can effectively realize the reuse of waste resources, solve the problem of large waste discharge and difficulty in handling, and meet the use needs of the building materials market. Further in the process of exploration, the solid waste raw materials, CO2-containing tail gas, and reactor device parameters were adjusted, and it was found that controlling the calcium hydroxide content in the solid waste within a certain range can promote the rapid release of heat energy by the mineralization reaction, and the temperature of the reaction system rises spontaneously. The temperature of the hydrothermal reaction is reached at the same time as the mineralization reaction, and the solid waste is fully utilized to effectively fix CO2, while the strength of the product is improved by the hydrothermal reaction. It is further found that when the content of the calcium-based component (calcium hydroxide and / or calcium oxide) of the Ca-based solid waste satisfies a certain relationship, the heat energy released by CO2 and mineralizable calcium in the reaction system can reach the optimal temperature of the hydrothermal reaction, so that the mineralization reaction and the hydrothermal reaction reach a balance, which on the one hand increases the carbon fixation rate of the building materials product, and on the other hand can keep the mechanical strength of the building materials product at a high level.

[0017] In some preferred embodiments, the step S1 specifically comprises firstly mixing the Ca-based solid waste with water to obtain a mixture (i.e., a reaction raw material), digesting and powder-mixing the mixture, and then molding the mixture to obtain a prefabricated building material.

[0018] More preferably, the solid-liquid ratio of the raw material of Ca-based solid waste to water is 1:(0.05-0.3).

[0019] In some preferred embodiments, the molding method is: transferring the material into a mold and applying a certain pressure to form a preformed building material; further preferably, the molding pressure is 5-110 MPa.

[0020] In some preferred embodiments, the S2 step is specifically to transfer the prefabricated building material to a reactor, introduce CO2-containing gas to carry out a composite mineralization reaction (the so-called composite mineralization reaction means not a simple mineralization reaction, in this system, both a mineralization reaction and a hydrothermal reaction occur), and obtain a high-strength building material product after reacting for 1-8 hours.

[0021] Further preferably, the pressure of the composite mineralization reaction in step S2 is 0.05-1 MPa.

[0022] More preferably, the filling rate when transferring the prefabricated building material product to the reactor is 10-60%; even more preferably, the filling rate is 15-50%.

[0023] In some preferred embodiments, the method for regenerating high-strength negative carbon building materials from Ca-based solid waste satisfies the following formula:

[0024] a>[H+3.593*10 5 *v / T0-3.593*m*10 8 / (T0*ρ)+4.446*v*10 5 *(P-37.315 / T0)-4.446*m*10 8 (P-37.315 / T0) / ρ+1.321*10 6 *m-4.864*10 6 *P+2.344*10 8 / (373.15-T0)-2.344*10 11 *m / (373.15*ρ*v-T0*ρ*v)] / [1.538*10 9 *m*k / (373.15-T0)-4.1*10 5 *m-9.86*10 5 *m*k];

[0025] Where: m is the mass of the building material prefabricated product, in t; H is the heat capacity of the reactor, in J / K; v is the volume of the reactor, in m 3 ρ is the true density of the building material prefabricated product (True density refers to the actual mass of solid matter per unit volume in an absolutely dense state, that is, the density after removing the internal pores or gaps between particles), the unit is kg / m 3 ; T0 is the initial reaction temperature, unit is K; P is the reaction pressure, unit is MPa; a is the mass fraction of calcium-based components in the reaction raw materials (the total mass fraction of calcium hydroxide in the embodiment of the present application), unit is %; k is the empirical reaction constant, unit is 1.

[0026] During the calculation process, the above parameters are substituted into the formula according to the above units and numerical calculations are performed. The units do not participate in the calculations.

[0027] Said Where Mi is the mass of each component of the reactor body M1, M2, M3...M n , Ci is the specific heat capacity C1, C2, C3...C corresponding to each component of the reactor n .

[0028] The materials of the reaction device are composed of a kettle body and a thermal insulation material, wherein the kettle body material can be one or more of carbon manganese steel, stainless steel, zirconium, nickel-based (Hastelloy, Monel) alloy and other composite materials; the thermal insulation material can be one or more of rare earth thermal insulation material, rock wool, inorganic silicate slurry, new inorganic thermal insulation material, polystyrene board, polyurethane foam material, glass wool, aluminum silicate wool and the like.

[0029] In some preferred embodiments, the method for regenerating high-strength negative carbon building materials from Ca-based solid waste also satisfies the following formula:

[0030] a<[H+3.593*10 5 *v / T0-3.593*m*10 8 / (T0*ρ)+4.446*v*10 5 *(P-47.315 / T0)-4.446*m*10 8 (P-47.315 / T0) / ρ+1.361*10 6 *m-3.453*10 6 *P+2.344*10 8 / (473.15-T0)-2.344*10 11 *m / (473.15*ρ*v-T0*ρ*v)] / [1.531*10 9*m*k / (473.15-T0)-4.1*10 5 *m-9.86*10 5 *m*k]; the value range of k is 0.8-1.

[0031] Further preferably, the numerical range of k is 0.84-1.

[0032] In some preferred embodiments, in the S2 step, the CO2-containing gas comes from industrial tail gas, and the volume fraction of CO2 in the industrial tail gas is 5-98%; further preferably, the volume fraction of CO2 in the industrial tail gas is 8-95%.

[0033] In some preferred embodiments, the industrial tail gas includes a mixture of one or more of chemical plant flue gas, cement plant flue gas, coal-fired power plant flue gas, lime kiln flue gas, steel plant flue gas, and carbon capture and analysis gas.

[0034] A second aspect of the present invention provides an application of a method for regenerating high-strength negative carbon building materials using Ca-based solid waste in the field of building materials.

[0035] Beneficial effects:

[0036] The method for regenerating high-strength negative carbon building materials from Ca-based solid waste provided in this application has the following advantages:

[0037] (1) The present invention makes full use of the large amount of reaction heat generated when calcium hydroxide in Ca-based solid waste fixes CO2, and synergistically prepares building materials with good carbon fixation performance and excellent physical properties, which greatly reduces the cost of solid waste disposal. On the one hand, it is beneficial to the recovery and utilization of tail gas in various high-carbon emission industries, and on the other hand, it solves the problem of disposing of large amounts of solid waste, which is beneficial to the resource development of the industry;

[0038] (2) In the method of regenerating high-strength negative carbon building materials from Ca-based solid waste, the present invention effectively utilizes the active calcium component in the solid waste to control the reaction heat release, improves the carbon fixation performance of the mineralized product, and at the same time makes the temperature in the system reach the temperature required for the hydration reaction, so that the product undergoes a hydration reaction in the later stage of the mineralization reaction, further improving the mechanical strength of the product, not only absorbing the waste CO2 in industrial production, but also avoiding the loss of excessive active components, further reducing the cost of building materials, and making full use of solid waste to convert it into high-strength building materials with excellent performance;

[0039] (3) The present invention uses pure bulk solid waste as raw material, directly introduces CO2 source gas into the reactor for mineralization and curing, and finds that under the control of specific process parameters, high-quality building materials can be produced, which can meet the large-scale use needs of the building materials industry to a great extent, and has extremely high promotion and application value;

[0040] (4) The present invention effectively realizes the efficient resource utilization of industrial solid waste. The total carbon emissions of the prepared building materials products are more than 50% lower than those of traditional silicate cement products, which plays an important role in promoting the low-carbon development of my country's building materials industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 is the glass transition temperature diagram of carbide slag;

[0042] Figure 2 Comparison of TG / DTG thermogravimetric analysis curves of Examples 2, 6, and 7;

[0043] Figure 3 This is the SEM image of Example 2. DETAILED DESCRIPTION

[0044] Examples 1-8

[0045] A method for regenerating high-strength negative carbon building materials from Ca-based solid waste is provided, comprising the following steps:

[0046] S1. Using Ca-based solid waste to prepare building material prefabricated products;

[0047] S2. Transfer the prefabricated building materials to a reactor, introduce CO2-containing gas to carry out a composite mineralization reaction, and obtain a high-strength negative carbon building material product.

[0048] Specifically, the step S1 is to uniformly mix the Ca-based solid waste with water to obtain a mixture, transfer the mixture to a digestion system for digestion for 40 minutes, and then send it to a mechanical forming system to be pressed into blocks at a forming pressure of 10 MPa. The specifications of the prefabricated building materials are 200 mm*95 mm*53 mm.

[0049] Specifically, the S2 step is to transfer 90.6t of building material preforms to a reactor (with a filling rate of 30%), introduce CO2-containing gas to carry out a composite mineralization reaction, wherein the initial temperature of the composite mineralization reaction is room temperature (25°C), the reaction time is 360min, the reaction pressure in the reactor is 0.6MPa, and the CO2 volume concentration is 76.5%. After the composite mineralization reaction is completed, a high-strength building material product is obtained.

[0050] The raw materials of the Ca-based solid waste include carbonized materials and auxiliary materials; the added amounts of carbonized materials, auxiliary materials and water in each embodiment and the content of calcium hydroxide in the raw materials of the Ca-based solid waste are shown in Table 1 (weight percentage).

[0051] The carbonized material is specifically carbide slag from a coal chemical plant, with a moisture content of 31.73%. The chemical composition and weight percentage of the XRF analysis are shown in Table 2; the auxiliary material uses two materials, auxiliary material one is specifically fly ash from a coal chemical plant, with a moisture content of 2%. The chemical composition and weight percentage of the XRF analysis are shown in Table 3; auxiliary material two is recycled material from a building materials factory, with a moisture content of 1%. The chemical composition and weight percentage of the XRF analysis are shown in Table 4.

[0052] In the S2 step, the CO2-containing gas comes from the tail gas produced by a salt-coal chemical plant in Hefei, and the composition of the tail gas is shown in Table 5.

[0053] The CaO and Ca(OH)2 listed in the following table have a conversion relationship. Taking the carbide slag containing 15.10% (Example 1) in the green body as an example, the moisture content of the carbide slag is 31.73%, and the content of the absolutely dry carbide slag is 10.31%. Figure 1 is the glass transition temperature diagram of carbide slag, wherein the mass reduction corresponding to 400-550°C represents the mass of water after the decomposition of calcium hydroxide, which accounts for 21.23%. The proportion of calcium hydroxide to carbide slag is 21.23% / 18*74=87.3%, and the percentage content of calcium hydroxide in carbide slag to the green body is 9.0% (due to XRF can only represent the composition of each element, and use oxides as the display form, but cannot represent the actual phase composition of the material, wherein CaO in the auxiliary material is inert calcium carbonate and does not participate in the reaction, therefore only the active calcium component in the carbide slag is calculated), i.e., a in Example 1 is 9.0%; similarly, a in Examples 2 to 8 are 11.0%, 13.5%, 17.0%, 18.0%, 20.1%, 25.0%, and 27.0%, respectively.

[0054] Table 1

[0055] Carbonized materials Supplementary material 1 Supplementary material 2 water Calcium hydroxide content Example 1 15.10% 36.35% 36.35% 12.20% 9.0% Example 2 18.45% 35.20% 35.20% 11.15% 11.0% Example 3 22.65% 33.77% 33.77% 9.81% 13.5% Example 4 28.52% 31.77% 31.77% 7.94% 17.0% Example 5 30.21% 31.19% 31.19% 7.41% 18.0% Example 6 33.69% 30% 30% 6.31% 20.0% Example 7 41.95% 26.61% 26.61% 3.16% 25.0% Example 8 45.30% 26.04% 26.04% 2.62% 27.0%

[0056] Table 2

[0057] Elemental composition CaO <![CDATA[CO2]]> <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[SO3]]> <![CDATA[Fe2O3]]> MgO <![CDATA[Na2O]]> LOSS content(%) 90.6 3.3 2.9 1.2 0.6 0.3 0.1 0.1 0.9

[0058] Table 3

[0059] Elemental composition <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[CO2]]> CaO <![CDATA[Fe2O3]]> <![CDATA[Na2O]]> <![CDATA[SO3]]> MgO LOSS content(%) 43.3 31.5 12.5 2.7 4.4 0.8 0.7 0.4 3.7

[0060] Table 4

[0061] Elemental composition <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[CO2]]> CaO <![CDATA[Fe2O3]]> <![CDATA[K2O]]> MgO <![CDATA[Na2O]]> LOSS content(%) 44.7 10.5 22.2 9.62 5.04 2.43 1.47 0.871 3.169

[0062] Table 5

[0063] Gas composition <![CDATA[CO2]]> <![CDATA[N2]]> SOx NOx VOCs Coal chemical tail gas 76.5% 18.9% 2.3% 2% 0.3%

[0064] The relevant information of the reactor, building material prefabricated products, etc. in step S2 is as follows:

[0065] The volume v of the reactor is 178.75m 3 , steel thickness 10mm, steel density 7950kg / m 3 , insulation rock wool thickness 100mm, rock wool density 120kg / m 3 ; H = 23345514 J / K; the true density of the prefabricated building material is 1690 kg / m 3 ; reaction pressure P is 0.6MPa; initial reaction temperature is 298.15K, mass of prefabricated building materials is 90.6t, and empirical reaction constant k is 1. During the calculation process, the above parameters are substituted into the formula according to the above units for numerical calculation, and the units are not involved in the calculation.

[0066] Substituting the above parameters into the formula, we obtain: 9.75%<a<25.55%.

[0067] Performance Testing Methods

[0068] 1. Compressive strength

[0069] The compressive strength of the finished high-strength building materials of Examples 1-8 was tested with reference to GBT4111-2013 "Test Methods for Concrete Blocks and Bricks". The strength of the test block was measured after natural air drying for 24 hours. The specific operation is as follows: The compression test uses a YE-30 hydraulic pressure testing machine. Five parallel samples are set for each high-strength building material product, and the average compressive strength of the parallel samples is calculated. If the difference between the measured sample compressive strength value and the average value is not greater than 15%, the average value is used as the compressive strength; if the difference between a certain measured value and the average value is greater than 15%, this value is discarded and the average value is calculated with the remaining values; if the difference between more than two measured values ​​and the average value is greater than 15%, the experiment is repeated. The test results are shown in Table 6.

[0070] The compressive strength can be calculated using the following formula: σD = P / F = 4P / πd 2 =P / 0.875d 2

[0071] Where σD——compressive strength, kgf / cm 2 ; P——crushing load, kgf; d——average diameter of particle sample, cm.

[0072] 2. Carbon fixation rate

[0073] The specific test steps for carbon fixation rate are as follows:

[0074] 1) Take 1 / 8 of the volume of the finished brick prepared in Example 1-10, crush it into powder and test the overall carbon fixation rate;

[0075] 2) Use a crusher to crush the powdered sample for the overall carbon fixation rate test. After crushing, take 50g of the sample and dry it in a 105℃ oven for 12h. Do not vacuum during drying, keep the oven closed, and place a large beaker of NaOH particles in the oven; after drying, take out 5g of the sample, grind it in a mortar until there is no granularity (about 1-2 minutes), and put it in a small ziplock bag; the small ziplock bag is placed in a large bag, and a silica gel desiccant is placed in the large bag.

[0076] 3) Place the prepared sample in the sample chamber, set the experimental atmosphere to N2, the temperature range to room temperature to 1000°C, and the heating rate to 10°C / min. Use the STA409EP comprehensive thermal analyzer manufactured by NETZSCH of Germany for testing and analysis; the test results are shown in Table 6;

[0077] 4) After the test, the TG / DTG thermogravimetric analysis curve is obtained; the TG / DTG thermogravimetric analysis curves of Examples 2, 6, and 8 are compared as shown in Figure 1 .

[0078] Note: This application uses the CO2 absorption rate to evaluate the carbon absorption effect of the sample, which is the percentage of the mass of CO2 absorbed by solid waste to the mass of the test block. The content of CO2 absorbed by solid waste is obtained by testing the TG / DTG thermogravimetric analysis curve of the mineralized product. The content of carbon dioxide absorbed by the mineralized product is the mass reduction at 605-820℃, and the mass of the test block is the mass of the mineralized product at 105℃.

[0079] Performance test data

[0080] Table 6

[0081]

[0082]

[0083] It can be seen from Table 6 that when the mass fraction of the calcium-based component (i.e., calcium hydroxide in the embodiments) in the reaction raw materials of embodiments 2-7 (i.e., the mixture used to prepare the prefabricated building materials) is within the range of the calculation results according to the formula of this application (9.75%<a<25.55%), the compressive strength and carbon fixation rate of the prepared finished building materials are relatively high. In embodiment 1, since its calcium hydroxide content is 9%, which is lower than the range specified by the formula calculation results, the compressive strength and carbon fixation rate of the prepared finished building materials are significantly lower than those of other embodiments. In embodiment 8, the calcium hydroxide content reaches 27%, which is higher than the range specified by the formula calculation results. Although a very high compressive strength is obtained, the carbon fixation rate is poor. This shows that mixing the ingredients according to the calculation results of the formula of this application is helpful to obtain building materials with high compressive strength and carbon fixation rate.

[0084] From Table 6, it can be seen that the calcium content of Example 1 did not reach the minimum limit, and the compressive strength and carbon fixation rate of the finished building material were relatively low; the carbon fixation rate of Examples 2-3 increased rapidly with the increase of the carbide slag content, and the strength of the finished building material increased rapidly with the increase of the carbide slag content; this is because, on the one hand, the increase in the mineralizable calcium content in the green body increases the theoretical amount of carbon that can be fixed in the finished building material, and on the other hand, the increase in the temperature of the reactor and the increase in the disturbance of the carbon dioxide gas increase the probability of contact with the mineralizable calcium, resulting in an increase in the carbon fixation rate, but the mineralized calcium carbonate has limited effect on the material strength, so the compressive strength increases slowly, and the low ambient temperature leads to less hydrothermal reaction in the system, and the strength of the test block is not significantly improved; the carbon fixation rate of Examples 4-6 increases with the increase of the carbide slag content The increase gradually slows down, and the product strength increases rapidly. This is because the increase in calcium content makes the reactor temperature reach a certain temperature, and the hydroxide destroys the silicon-oxygen bond and aluminum-oxygen bond in the silicon-aluminum solid waste. At the same time, the generated silicate ions combine with calcium ions to form CSH gel / Tobermorite, which makes the product strength increase rapidly, and the carbon fixation rate increases slowly; in Examples 7-8, as the calcium content increases rapidly, the carbon fixation rate of the finished building materials decreases significantly. This is because the increase in the mineralizable calcium content makes the mineralization degree higher in the initial stage of the reaction, the temperature rise in the reactor is large, and after reaching a certain temperature, a large amount of remaining calcium hydroxide and calcium oxide reacts hydrothermally with silicon-aluminum to generate a large amount of CSH, and the mineralizable calcium hydroxide and calcium oxide decrease rapidly, which reduces the carbon fixation rate and significantly improves the compressive strength.

[0085] To further prove the above conjecture, the applicant has carried out structural characterization on the building materials generated in Example 2, such as Figure 3 shown. Figure 3 This is the SEM image of the product prepared in Example 2. From the figure, it can be seen that there is a needle-shaped tobermorite structure in the product, which is the same as the hydrothermally generated tobermorite crystal structure reported in the prior art (for example, "Application of hydrothermal solidification technology of ceramic waste in indoor thin plate materials"). It means that the heat released by the mineralization of this application has reached the required hydrothermal conditions, and the silicon-calcium substances in the raw materials have undergone hydrothermal reaction to generate tobermorite crystals, further enhancing the strength of the product.

Claims

1. A method for regenerating high-strength negative carbon building materials from Ca-based solid waste, characterized in that: The degree of mineralization reaction in the system is controlled by controlling the mineralizable calcium content in the reaction raw materials, and the temperature of the system is regulated by utilizing the heat released by the mineralization reaction to achieve the conditions required for the hydrothermal reaction, so that both the mineralization reaction and the hydrothermal reaction can be carried out in the system, thereby producing high-strength building materials. The method for regenerating high-strength negative carbon building materials from Ca-based solid waste satisfies the following formula: a>[H+3.593*10 5 *v / T0-3.593*m*10 8 / (T0*ρ)+4.446*v*10 5 *(P-37.315 / T0)-4.446*m*10 8 (P-37.315 / T0) / ρ+1.321*10 6 *m-4.864*10 6 *P+2.344*10 8 / (373.15-T0)-2.344*10 11 *m / (373.15*ρ*v-T0*ρ*v)] / [1.538*10 9 *m*k / (373.15-T0)-4.1*10 5 *m-9.86*10 5 *m*k]; The method for regenerating high-strength negative carbon building materials from Ca-based solid waste also satisfies the following formula: a<[H+3.593*10 5 *v / T0-3.593*m*10 8 / (T0*ρ)+4.446*v*10 5 *(P-47.315 / T0)-4.446*m*10 8 (P-47.315 / T0) / ρ+1.361*10 6 *m-3.453*10 6 *P+2.344*10 8 / (473.15-T0)-2.344*10 11 *m / (473.15*ρ*v-T0*ρ*v)] / [1.531*10 9 *m*k / (473.15-T0)-4.1*10 5 *m-9.86*10 5 *m*k]; The value range of k is 0.8-1; Where: m is the mass of the building material prefabricated product, in t; H is the heat capacity of the reactor, in J / K; v is the volume of the reactor, in m 3 ; ρ is the true density of the prefabricated building material, in kg / m 3 ; T0 is the initial temperature of the reaction, unit is K; P is the reaction pressure, unit is MPa; a is the mass fraction of calcium-based components in the reaction raw materials, unit is %; k is the empirical reaction constant, unit is 1; The method for regenerating high-strength negative carbon building materials from Ca-based solid waste does not use an external heat source or additional water vapor. The method for regenerating high-strength negative carbon building materials from Ca-based solid waste comprises the following steps: S1. Preparing building material preforms using Ca-based solid waste; S2. The prefabricated building materials are transferred to a reactor, and CO2-containing gas is introduced to carry out a composite mineralization reaction to obtain a high-strength negative carbon building material product.

2. The method for regenerating high-strength negative carbon building materials from Ca-based solid waste according to claim 1, characterized in that: The raw materials of the Ca-based solid waste include carbonized materials and auxiliary materials; the carbonized materials include one or more of carbide slag, white mud, and fly ash; the auxiliary materials include one or more of fly ash, bottom ash, red mud, construction waste, waste cement, tailings, and ore raw materials.

3. The method for regenerating high-strength negative carbon building materials from Ca-based solid waste according to claim 2, characterized in that: The mass fraction of the calcium-based component in the carbonized material is not less than 80%.

4. The method for regenerating high-strength negative carbon building materials from Ca-based solid waste according to claim 1, characterized in that: The step S1 specifically comprises: uniformly mixing the Ca-based solid waste with water to obtain a mixture, digesting and powder-mixing the mixture, and then molding the mixture to obtain a prefabricated building material.

5. The method for regenerating high-strength negative carbon building materials from Ca-based solid waste according to claim 1, characterized in that: In step S2, the CO2-containing gas comes from industrial tail gas, and the volume fraction of CO2 in the industrial tail gas is 5-98%.

6. Application of the method for regenerating high-strength negative carbon building materials from Ca-based solid waste according to any one of claims 1 to 5 in the field of building materials.