A binary metal alloy catalyst and its preparation method and application
The preparation of binary metal alloy catalysts through rapid chemical co-deposition and gentle heat treatment has solved the problem of slow hydrogen analysis rate of electrolytic water in alkaline media and scarce precious metal resources, and achieved efficient hydrogen generation and low-cost catalyst preparation, which significantly improved Electrochemical activity of alkaline hydrogen evolution reaction.
Patent Information
- Application Number
- CN202211394376.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-08
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-11-08
AI Technical Summary
In alkaline media, the kinetic rate of electrolytic hydrogen evolution reaction is slow, and precious metal resources are scarce. The degree of alloying in the prior art is insufficient, resulting in high catalyst preparation cost.
The binary metal alloy catalyst is prepared by rapid chemical co-deposition and gentle heat treatment. By synchronously reducing precious metals and non-precious metal precursors in excess reducing agents, a partially crystallized binary alloy catalyst is formed, which increases the degree of alloying and reduces precious metals. Use amount.
The acceleration of the hydrolysis reaction under an alkaline medium is achieved, the efficiency of hydrogen generation is improved, the cost of catalyst preparation is reduced, and excellent electrochemical mass activity is shown in the alkaline hydrogen evolution reaction.
Smart Images

Figure CN115846675B_ABST
Abstract
Description
Technical field:
[0001] The present invention relates to the technical field of electrocatalysis, and in particular to a binary metal alloy catalyst and a preparation method and application thereof. Background technology:
[0002] As global climate and environmental problems intensify year by year, the energy revolution advocating the development of new green renewable energy as the main carrier has quietly started. Fossil fuels, which used to be the main energy form, are slowly being replaced by new energy forms, such as solar energy, wind energy, and hydrogen energy. Among them, hydrogen energy products only produce water, with no carbon emissions. At the same time, it can effectively store intermittent energy forms such as solar energy and wind energy, and is a very valuable green energy carrier. The production of hydrogen currently relies mainly on steam reforming of natural gas, which not only consumes extra energy, but also produces a large amount of greenhouse gases, which puts pressure on the environment; and the electrolysis of water can not only realize the production of pure hydrogen, but also realize the storage and re-conversion of the above intermittent energy in the form of electricity. Therefore, water electrolysis technology is one of the most promising ways to produce hydrogen in the future. Since alkaline media have a relatively mild chemical environment for electrode materials compared to acidic media, it can provide potential guarantees for materials to obtain more ideal electrocatalytic activity and stability. Therefore, the development of water electrolysis technology in alkaline environment has attracted more and more attention. However, in alkaline medium, the kinetic rate of the electrolytic water hydrogen evolution reaction is much slower than the rate under the corresponding acidic medium, and this is also true for the noble metal platinum. Therefore, it is crucial to try to improve the kinetic reaction rate of the water dissociation step. Considering the scarcity of precious metal resources, by alloying the precious metal with the high-abundance transition metal to prepare the catalytic material, not only can the kinetic reaction rate of hydrogen evolution under alkaline medium be improved to a great extent, but also the preparation cost of the catalyst can be reduced by controlling the usage of the precious metal. Regarding the preparation of platinum-containing binary metal alloy catalysts, in the prior art, such as CN1774827A (fuel cell supported catalyst, method for manufacturing the catalyst and fuel cell), two metal salts are added to the solution step by step, and the reducing agent used by each is also added step by step, so that the two metal salts are metallized step by step during the solution reduction process, and no alloying process is produced, which is only realized in the subsequent high-temperature pyrolysis process; at the same time, due to the process of adding and reducing the two metal salts step by step in the technology, the degree of alloying is not enough. Summary of the invention:
[0003] The present invention solves the problems existing in the prior art and provides a binary metal catalyst and a preparation method and application thereof. The present invention realizes the preparation of the binary metal alloy catalyst through a simple strategy of rapid chemical co-deposition / mild heat treatment, wherein the amorphous structure provides a favorable spatial site for the adsorption of water molecules and water dissociation intermediates in an alkaline medium, and the formation of a non-precious metal / precious metal binary alloy structure makes the surface rich in high-valent metal species, and the two synergistically promote the dissociation of water and the generation of hydrogen.
[0004] The purpose of the present invention is to provide a method for preparing a binary metal alloy catalyst, comprising the following steps: dispersing a conductive carrier in water, adding an excess reducing agent and stirring until fully dissolved to obtain a mixed solution A; dissolving a noble metal precursor and a non-noble metal precursor in water to prepare a mixed solution B, and then adding the mixed solution B dropwise to the mixed solution A, stirring at room temperature, centrifuging and washing to remove the supernatant, drying the precipitated product, and heat treating it in a hydrogen-argon mixed atmosphere, and after the temperature drops to room temperature, the obtained product is the binary metal alloy catalyst. The preparation method is simple to operate, green and pollution-free, low in cost, and can achieve batch preparation.
[0005] The present invention, on the one hand, prepares two metal salts into a mixed solution first, so as to achieve the simultaneous reduction of the two metals in the subsequent liquid phase reduction process, thereby improving the alloying degree of the two metals; on the other hand, unlike the previous preparation technology of adding the reducing agent dropwise into the metal salt solution for a gentle reduction, the present invention adopts a reverse rapid reduction strategy, adding the two metal salt mixed solution into the excess reducing agent, first preparing an amorphous alloy, and then further heat treating under a reducing atmosphere to obtain a partially crystallized binary alloy catalyst. The partially crystallized binary alloy catalyst prepared by the present invention still contains a large amount of amorphous structure because only a partial crystallization treatment is performed, which is very beneficial for the adsorption of intermediate species in the alkaline hydrogen evolution reaction, which is obviously different from the binary metal alloy catalyst prepared in the previous technical invention.
[0006] Preferably, the preparation method specifically comprises the following steps: dispersing the carbon carrier in deionized water, adding an excess reducing agent and stirring at room temperature to obtain a mixed solution A, dissolving a platinum-containing precursor compound and a nickel-containing precursor compound in deionized water to prepare a mixed solution B, wherein the molar ratio of platinum to nickel in the mixed solution B is 1:1 to 1:10, and the molar ratio of the reducing agent in the mixed solution A to the metal in the mixed solution B is 5:1 to 12:1, and the mixed solution B is added dropwise to the mixed solution A, stirred at room temperature for 0.3-1.0h, centrifuged and washed to remove the supernatant, and after the precipitated product is dried, heat treated at 300°C to 700°C in a hydrogen-argon mixed atmosphere for 0.5 to 2 hours, the volume percentage of hydrogen in the hydrogen-argon mixed atmosphere is 5% to 20%, and after the temperature drops to room temperature, the obtained product is the binary metal alloy catalyst. The molar ratio of the metal in the mixed solution B refers to the sum of the molar ratios of platinum and nickel.
[0007] More preferably, the carbon carrier is selected from one of carbon black (XC-72R), expanded graphite, graphene oxide, acetylene black and carbon nanotubes.
[0008] Further preferably, the platinum-containing precursor compound is selected from at least one of potassium chloroplatinate, ammonium chloroplatinite, chloroplatinic acid and potassium chloroplatinite, and the nickel-containing precursor compound is selected from at least one of nickel chloride hexahydrate, nickel acetate tetrahydrate, nickel nitrate hexahydrate and nickel sulfate hexahydrate.
[0009] More preferably, the molar ratio of platinum to nickel in the mixed solution B is 1:10, and the molar ratio of the reducing agent in the mixed solution A to the metal in the mixed solution B is 9-10:1.
[0010] More preferably, the volume percentage of hydrogen in the hydrogen-argon mixed atmosphere is 5%, the heat treatment temperature is 400° C., and the heat treatment time is 1 hour.
[0011] Preferably, the reducing agent is selected from one of sodium borohydride, potassium borohydride, hydrazine hydrate and thiourea dioxide.
[0012] The present invention also protects a binary metal alloy catalyst prepared by the above preparation method, which is composed of partially crystallized alloy nanoparticles composed of precious metals and non-precious metals loaded on a conductive carrier, wherein the particle size of the binary metal alloy nanoparticles ranges from 2 to 10 nm, the loading amount of the precious metal is 2 to 10 wt.%, and the molar ratio of the precious metal to the non-precious metal is 1:1 to 1:10. The partially crystallized binary metal alloy includes two organizational forms, crystalline and amorphous.
[0013] The present invention also protects the application of the above binary metal alloy catalyst, specifically the application of the binary metal alloy catalyst in the catalysis of hydrogen evolution reaction by electrolysis of water in an alkaline environment. The binary metal alloy catalyst proposed by the present invention has a certain degree of amorphous microstructure on its surface, which can provide a favorable adsorption energy barrier for water molecules and water dissociation intermediate species in alkaline media, and the alloy structure can accelerate the reaction kinetics of the water dissociation process, and exhibits excellent electrochemical mass activity in the catalysis of hydrogen evolution by alkaline water electrolysis, especially at high current density.
[0014] Compared with the prior art, the present invention has the following advantages:
[0015] 1. The present invention realizes the preparation of binary metal alloy catalysts through a simple strategy of rapid chemical co-deposition / mild heat treatment, wherein the amorphous structure provides favorable spatial sites for the adsorption of water molecules and water dissociation intermediates in alkaline media, and the formation of non-precious metal / precious metal binary alloy structure makes the surface rich in high-valent metal species, which synergistically promote the dissociation of water and the generation of hydrogen. The alloy nanoparticles are evenly distributed on the surface of the carrier, and the particle size distribution is uniform, providing abundant active sites for the alkaline hydrogen evolution reaction.
[0016] 2. The present invention can effectively reduce the usage of precious metals and improve the utilization efficiency of precious metals by alloying precious metals with non-precious metals, and exhibit excellent mass activity in alkaline hydrogen evolution reaction. It is significantly better than commercial platinum carbon under the same metal loading and electrochemical test conditions.
[0017] 3. The preparation process adopted by the binary metal alloy catalyst proposed in the present invention has simple operation procedures, is green and pollution-free, has low cost, and can be prepared in batches. Description of the drawings:
[0018] Figure 1 XRD patterns of the binary metal alloy catalysts prepared in Examples 1-8 and Comparative Examples 1-2;
[0019] Figure 2 a and Figure 2 b are SEM backscattered electron images of the binary metal alloy catalysts prepared in Example 1 and Comparative Example 1, respectively;
[0020] Figure 3 a is a TEM morphology of the binary metal alloy catalyst prepared in Example 1, Figure 3 b is the particle size distribution histogram of the nanoparticles, Figure 3 c is the selected area electron diffraction pattern;
[0021] Figure 4 a is the linear sweep voltammetry curve of the catalyst in Examples 1-8 and Comparative Examples 1-4, Figure 4 b is the current density of the corresponding sample at 10 mA cm -2 The overpotential value at . Specific implementation method:
[0022] The following examples are provided to further illustrate the present invention, rather than to limit the present invention.
[0023] Unless otherwise defined, all professional terms used hereinafter have the same meaning as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specified, the experimental materials and reagents herein are conventional commercial products in the art.
[0024] The present invention provides a binary metal alloy catalyst, which consists of a conductive carrier and binary metal alloy nanoparticles loaded thereon, the binary metal alloy nanoparticles have a particle size of 2 to 10 nm, the loading amount of platinum in the catalyst is 2 to 10 wt.%, and the molar ratio of precious metals to non-precious metals is 1:1 to 1:10.
[0025] The preparation method of a binary metal alloy catalyst specifically comprises the following steps: dispersing a carbon carrier in deionized water, adding an excess reducing agent and stirring at room temperature until fully dissolved to obtain a mixed solution A; dissolving a platinum-containing precursor compound and a nickel-containing precursor compound in deionized water to prepare a mixed solution B, and then adding the mixed solution B dropwise into the mixed solution A, stirring at room temperature for a period of time, centrifuging and washing, removing the supernatant, collecting the precipitated product, vacuum drying, and heat treating it at a certain temperature in a hydrogen-argon mixed atmosphere for a period of time, and after the temperature drops to room temperature, the binary metal alloy catalyst is obtained.
[0026] There is no particular restriction on the source of the carbon carrier raw material in the present invention, and commercially available products known to those skilled in the art can be used. In the following embodiments, preferably, the carbon carrier is selected from one of carbon black (XC-72R), expanded graphite, graphene oxide, acetylene black and carbon nanotubes.
[0027] In the present invention, the molar ratio of platinum to nickel in the platinum-containing precursor compound and the nickel-containing precursor compound is 1:1 to 1:10, preferably the molar ratio of metal in the noble metal and non-noble metal precursor molecules is 1:10, and the ratio of the reducing agent to the total amount of platinum and nickel in the platinum-containing precursor compound and the nickel-containing precursor compound is 5:1 to 12:1, preferably 9 to 10:1. In the following embodiments, the molar concentrations of the platinum-containing precursor compound and the nickel-containing precursor compound in the mixed solution B are both 0.25M.
[0028] In the present invention, there is no particular limitation on the source of the reducing agent, and commercially available products known to those skilled in the art can be used. In the following embodiments, preferably, the reducing agent is selected from one of sodium perborohydride, potassium borohydride, hydrazine hydrate and thiourea dioxide.
[0029] In the present invention, there is no particular restriction on the sources of the platinum-containing precursor compound and the nickel-containing precursor compound, and commercially available products known to those skilled in the art can be used. In the following embodiments, preferably, the platinum-containing precursor compound is selected from at least one of potassium chloroplatinate, ammonium chloroplatinite, chloroplatinic acid and potassium chloroplatinite, and the nickel-containing precursor compound is selected from at least one of nickel chloride hexahydrate, nickel acetate tetrahydrate, nickel nitrate hexahydrate and nickel sulfate hexahydrate.
[0030] In the present invention, the volume percentage of hydrogen in the hydrogen-argon mixed atmosphere is 5% to 20%, the heat treatment temperature is 300°C to 700°C, and the heat treatment time is 0.5 to 2 hours. It is more preferred that the volume percentage of hydrogen in the hydrogen-argon mixed atmosphere is 5%, the heat treatment temperature is 400°C, and the heat treatment time is 1 hour.
[0031] Example 1
[0032] Weigh 0.5 g of carbon black (XC-72R) and disperse it in 20 mL of deionized water. After stirring for 20 minutes, add 0.593 g of potassium borohydride until it is fully dissolved to form a mixed solution A. Dissolve potassium chloroplatinite (0.1 mmol) and nickel chloride hexahydrate (1 mmol) in water to form a mixed solution B. Then, add the mixed solution B dropwise into the mixed solution A and continue stirring at room temperature for half an hour. Collect the mixture after centrifugal washing, and then place it in a vacuum dryer at 80 ° C. Heat treat it at 400 ° C for 1 hour in a hydrogen and argon mixed atmosphere (the volume percentage of hydrogen is 5 vol.%). After naturally cooling to room temperature, the target catalyst Pt-Ni / C-1 is obtained.
[0033] The mass percentage of precious metal in Pt-Ni / C-1 is 3.27wt.%, and its XRD spectrum is shown in Figure 1 The diffraction peak is between the diffraction peaks of metal platinum and metal nickel, and is wider than the peak type, which means that an alloy phase structure is formed between metal nickel and metal platinum, and the degree of crystallization is low. Its TEM morphology, particle size statistics and selected area electron diffraction diagram are shown in Figure 1. Figure 3 As shown, from Figure 3 a It can be clearly observed that the metal nanoparticles are uniformly dispersed on the surface of the conductive carrier, and the corresponding particle size range is 8.0±1.8nm ( Figure 3 b), Figure 3 The obvious diffuse ring in c means that the degree of crystallization of the metal alloy phase is low.
[0034] Example 2
[0035] Weigh 0.5g of carbon black (XC-72R) and disperse it in 20mL of deionized water. After stirring for 20 minutes, add 0.107g of potassium borohydride until it is fully dissolved to form a mixed solution A. Potassium chloroplatinite (0.1mmol) and nickel chloride hexahydrate (0.1mmol) are prepared into a mixed solution B. Then, the mixed solution B is dropped into the mixed solution A, and stirring is continued at room temperature for half an hour. After centrifugal washing, the mixture is collected and then placed in a vacuum dryer at 80°C. It is heat treated at 400°C in a hydrogen-argon mixed atmosphere (the volume percentage of hydrogen is 5vol.%) for 1 hour. After naturally cooling to room temperature, the target catalyst Pt-Ni / C-2 is obtained.
[0036] Example 3
[0037] Weigh 0.5 g of carbon black (XC-72R) and disperse it in 20 mL of deionized water. After stirring for 20 minutes, add 0.269 g of potassium borohydride until it is fully dissolved to form a mixed solution A. Potassium chloroplatinite (0.1 mmol) and nickel chloride hexahydrate (0.4 mmol) are prepared into a mixed solution B. Then, solution B is dropped into solution A and continued to be stirred at room temperature for half an hour. After centrifugal washing, the mixture is collected and then placed in a vacuum dryer at 80 ° C. Heat treated at 400 ° C for 1 hour in a hydrogen-argon mixed atmosphere (the volume percentage of hydrogen is 5 vol.%). After naturally cooling to room temperature, the target catalyst Pt-Ni / C-3 is obtained.
[0038] Example 4
[0039] Weigh 0.5 g of acetylene black and disperse it in 20 mL of deionized water. After stirring for 20 minutes, add 0.593 g of potassium borohydride until it is fully dissolved to form a mixed solution A. Potassium chloroplatinate (0.1 mmol) and nickel nitrate hexahydrate (1 mmol) are prepared into a mixed solution B. Then, the mixed solution B is dropped into the mixed solution A, and stirring is continued at room temperature for half an hour. After centrifugal washing, the mixture is collected and then placed in a vacuum dryer at 80° C., and heat-treated at 400° C. for 1 hour in a hydrogen-argon mixed atmosphere (the volume percentage of hydrogen is 5 vol.%). After naturally cooling to room temperature, the target catalyst Pt-Ni / C-4 is obtained.
[0040] Example 5
[0041] Weigh 0.5 g of graphene oxide and disperse it in 20 mL of deionized water. After stirring for 20 minutes, add 0.593 g of potassium borohydride until it is fully dissolved to form a mixed solution A. Potassium chloroplatinate (0.1 mmol) and nickel acetate tetrahydrate (1 mmol) are prepared into a mixed solution B. Then, the mixed solution B is dropped into the mixed solution A, and stirring is continued at room temperature for half an hour. After centrifugal washing, the mixture is collected and then placed in a vacuum dryer at 80 ° C., and heat-treated at 500 ° C for 1 hour in a hydrogen-argon mixed atmosphere (the volume percentage of hydrogen is 5 vol.%). After naturally cooling to room temperature, the target catalyst Pt-Ni / C-5 is obtained.
[0042] Example 6
[0043] Weigh 0.5 g of carbon black (XC-72R) and disperse it in 20 mL of deionized water. After stirring for 20 minutes, add 0.593 g of sodium borohydride until it is fully dissolved to form a mixed solution A. Potassium chloroplatinite (0.1 mmol) and nickel chloride hexahydrate (0.1 mmol) are prepared into a mixed solution B. Then, the mixed solution B is dropped into the mixed solution A, and stirring is continued at room temperature for half an hour. The mixture is collected after centrifugal washing, and then placed in a vacuum dryer at 80 ° C. Heat treated at 600 ° C for 1 hour in a hydrogen-argon mixed atmosphere (the volume percentage of hydrogen is 5 vol.%). After naturally cooling to room temperature, the target catalyst Pt-Ni / C-6 is obtained.
[0044] Example 7
[0045] The present invention is the same as Example 1, except that the conductive carrier is carbon nanotubes, the precious metal and non-precious metal precursor molecules are chloroplatinic acid and nickel sulfate hexahydrate respectively, the molar ratio of the metals in the precious metal and non-precious metal precursor molecules is 1:10, the reducing agent is hydrazine hydrate, the molar ratio of the reducing agent to the metal is 12:1, the volume percentage of hydrogen in the hydrogen-argon atmosphere during the heat treatment is 5 vol.%, the heat treatment temperature is 700°C, the heat treatment time is 0.5 hour, and the target catalyst obtained is Pt-Ni / C-7.
[0046] Example 8
[0047] The same as Example 1, except that: the conductive carrier is expanded graphite, the precious metal and non-precious metal precursor molecules are ammonium chloroplatinite and nickel chloride hexahydrate, respectively, the molar ratio of the metal in the precious metal and non-precious metal precursor molecules is 1:1, the reducing agent is thiourea dioxide, the molar ratio of the reducing agent to the metal is 5:1, the volume percentage of hydrogen in the hydrogen-argon atmosphere during the heat treatment is 20 vol.%, the heat treatment temperature is 300°C, the heat treatment time is 2 hours, and the obtained target catalyst is Pt-Ni / C-8.
[0048] Comparative Example 1
[0049] Weigh 0.5 g of carbon black (XC-72R) and disperse it in 20 mL of deionized water. After stirring for 20 minutes, potassium chloroplatinite (0.1 mmol) and nickel chloride hexahydrate (1 mmol) are dissolved in water to form a mixed solution A. 0.593 g of potassium borohydride is added until fully dissolved to form a mixed solution B. Then, the mixed solution B is dropped into the mixed solution A, and stirring is continued at room temperature for half an hour. The mixture is collected after centrifugal washing, and then placed in a vacuum dryer at 80 ° C. Heat treated at 400 ° C for 1 hour in a hydrogen-argon mixed atmosphere (the volume percentage of hydrogen is 5 vol.%). After naturally cooling to room temperature, the target catalyst R-Pt-Ni / C is obtained.
[0050] from Figure 2 It can be seen from the backscattered electron image shown in b that compared with Example 1 ( Figure 2 a), the catalyst prepared by the method described in Comparative Example 1 tends to result in the generation of relatively large metal particles, thereby affecting its electrochemical hydrogen evolution activity.
[0051] Comparative Example 2
[0052] Weigh 0.5 g of carbon black (XC-72R) and disperse it in 20 mL of deionized water. After stirring for 20 minutes, add 0.593 g of potassium borohydride until it is fully dissolved to form a mixed solution. Dissolve potassium chloroplatinite (0.1 mmol) in 4 mL of deionized water and then drop it into the above mixed solution. Continue stirring at room temperature for half an hour, collect after centrifugal washing, and then place it in a vacuum dryer at 80 ° C. Heat treat it at 400 ° C in a hydrogen and argon mixed atmosphere (5 vol.%) for 1 hour. After it naturally cools to room temperature, the catalyst S-Pt / C is obtained.
[0053] Comparative Example 3
[0054] Weigh 0.5 g of carbon black (XC-72R) and disperse it in 20 mL of deionized water. After stirring for 20 minutes, add 0.593 g of potassium borohydride until it is fully dissolved to form a mixed solution. Dissolve nickel chloride hexahydrate (1 mmol) in 4 mL of deionized water and then drop it into the above mixed solution. Continue stirring at room temperature for half an hour, collect after centrifugal washing, and then place it in a vacuum dryer at 80°C. Heat treat it at 400°C in a hydrogen and argon mixed atmosphere (5 vol.%) for 1 hour. After naturally cooling to room temperature, the catalyst S-Ni / C is obtained.
[0055] Comparative Example 4
[0056] Commercial platinum-on-carbon catalyst (20 wt. %) was purchased from Johnson Matthey.
[0057] In an argon-saturated 1 M KOH electrolyte solution, the hydrogen evolution activity of the catalysts in Examples 1-8 and Comparative Examples 1-4 was evaluated by linear sweep voltammetry. Figure 4 As shown. Figure 4 It can be seen that in the argon-saturated 1M KOH electrolyte solution, the catalyst Pt-Ni / C-1 prepared in Example 1 has a current density of 10 mA cm -2 When the overpotential is 100 mV, the mass activity is Better than the values of the catalysts in other examples (Examples 2-8) and comparative examples (Comparative Examples 1-4) under the same test conditions, at low noble metal loading It exhibits excellent alkaline hydrogen evolution activity.
[0058] The description of the above embodiments is only used to help understand the technical solution and core ideas of the present invention. It should be pointed out that for technicians in this technical field, several improvements and modifications can be made to the present invention without departing from the principles of the present invention. These improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A binary metal alloy catalyst, It is characterized in that The invention is composed of partially crystallized alloy nanoparticles composed of precious metals and non-precious metals loaded on a conductive carrier, wherein the particle size of the binary metal alloy nanoparticles is in the range of 2-10 nm, the loading amount of the precious metal is in the range of 2-10 wt.%, and the molar ratio of the precious metal to the non-precious metal is in the range of 1:1-1:10; the preparation method of the binary metal alloy catalyst comprises the following steps: dispersing a carbon carrier in deionized water, adding an excess reducing agent, stirring at room temperature to obtain a mixed solution A, dissolving a platinum-containing precursor compound and a nickel-containing precursor compound in deionized water to obtain a mixed solution B, wherein the molar ratio of platinum to nickel in the mixed solution B is in the range of 1:1-1:10, and the molar ratio of the reducing agent in the mixed solution A to the metal in the mixed solution B is in the range of 5:1-12:1, and adding the mixed solution B dropwise into the mixed solution A, stirring at room temperature for 0.3-1.0 h later, the supernatant is removed by centrifugal washing, the precipitated product is dried, and then heat treated at 300°C to 700°C for 0.5 to 2 hours in a hydrogen-argon mixed atmosphere, wherein the volume percentage of hydrogen in the hydrogen-argon mixed atmosphere is 5% to 20%. After the temperature drops to room temperature, the obtained product is the binary metal alloy catalyst.
2. The binary metal alloy catalyst according to claim 1, It is characterized in that The carbon carrier is selected from one of carbon black, expanded graphite, graphene oxide, acetylene black and carbon nanotubes.
3. The binary metal alloy catalyst according to claim 1, It is characterized in that The platinum-containing precursor compound is selected from at least one of potassium chloroplatinate, ammonium chloroplatinite, chloroplatinic acid and potassium chloroplatinite, and the nickel-containing precursor compound is selected from at least one of nickel chloride hexahydrate, nickel acetate tetrahydrate, nickel nitrate hexahydrate and nickel sulfate hexahydrate.
4. The binary metal alloy catalyst according to claim 1, It is characterized in that The molar ratio of platinum to nickel in the mixed solution B is 1:10, and the molar ratio of the reducing agent in the mixed solution A to the metal in the mixed solution B is 9-10:
1.
5. The binary metal alloy catalyst according to claim 1, It is characterized in that The volume percentage of hydrogen in the hydrogen-argon mixed atmosphere is 5%, the heat treatment temperature is 400° C., and the heat treatment time is 1 hour.
6. The binary metal alloy catalyst according to claim 1, It is characterized in that The reducing agent is selected from one of sodium borohydride, potassium borohydride, hydrazine hydrate and thiourea dioxide.
7. Use of the binary metal alloy catalyst according to claim 1, It is characterized in that The binary metal alloy catalyst is used for catalyzing the hydrogen evolution reaction of water electrolysis in an alkaline environment.