Transition metal wastewater treatment method and transition metal recovery method
The photocatalytic system oxidizes the nickel complex under light and electricity, which solves the problem of nickel complex wastewater treatment in the existing technology, achieves efficient removal and recovery of nickel, reduces power consumption, and reduces pollutant transfer.
Patent Information
- Application Number
- CN202211710981.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-12-29
AI Technical Summary
Existing technology is difficult to effectively remove heavy metals in nickel complex wastewater, making it difficult to degrade and transfer pollutants, affecting the environment and health.
Using a photocatalytic system, the conductive glass anode loaded with titanium dioxide nanorod arrays is used to generate strong oxidizing photogenerated holes under light and electricity, which oxidizes and adsorbs transition metals on the anode surface, thereby achieving selective removal and enrichment, and Transition metals are recovered by reverse current flow or acid solution.
It achieves efficient decomposition and removal of nickel complexes, reduces power consumption, improves the processing efficiency of transition metal ions, realizes direct recovery of nickel, and reduces secondary pollution.
Smart Images

Figure CN115849518B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sewage treatment, and in particular to a transition metal sewage treatment method and a transition metal recovery method. Background Art
[0002] Nickel has the characteristics of high mechanical strength, corrosion resistance, good ductility, and high chemical stability. Electroplated nickel can form a stable coating on the surface of the plated part, which has an ideal protective effect. Its structure is compact and delicate, with strong corrosion resistance and excellent wear resistance. It is widely used in the industrial industry. At the same time, a large amount of chelating agents are often required in the production process of the nickel electroplating industry, and the heavy metal substances in its wastewater mainly exist in a complex state. Compared with free heavy metal nickel, the complexed heavy metal nickel is firmly bound to the ligand of the chelating agent and is difficult to be effectively removed by traditional heavy metal treatment technologies such as alkaline precipitation, ion exchange and adsorption. Taking Ni(Ⅱ)-EDTA as an example, flocculation and ion exchange can only remove 5% of the metal complexes, while membrane filtration and electrodialysis technology can only concentrate the sewage, and cannot truly achieve the effective removal of Ni(Ⅱ)-EDTA, and will also produce secondary pollutants such as high-concentration metal complex concentrates. At the same time, due to its high stability, metal nickel complexes are difficult to be intercepted by soil and sediments, and have higher migration ability and long-distance transmission ability in the water environment than free metal ions. Excessive nickel in the water environment can affect the growth and development of plants, and even lead to the death of plants; excessive intake of nickel-containing substances can lead to nickel poisoning, which can cause serious diseases such as dermatitis, respiratory cancer and degeneration of the human nervous system. Studies have shown that metal complexes can further enhance the biological toxicity of heavy metals to biological cells, bacteria and plants. When nickel complexes enter the water environment, they can remain in the water environment for a long time due to their difficulty in biodegradation and high stability, and accumulate and transfer in the food chain through bioaccumulation, thus bringing lasting and far-reaching impacts on the ecological environment and human health. Therefore, the development of new nickel complex wastewater treatment technology to achieve efficient and low-consumption treatment and resource utilization of nickel complex wastewater not only has scientific research value, but also has great environmental significance. Summary of the invention
[0003] In order to overcome the problem that the prior art cannot effectively treat nickel complex wastewater, the first aspect of the present invention provides a transition metal wastewater treatment method, and the second aspect of the present invention provides a transition metal recovery method.
[0004] In order to achieve the above object, the technical solution adopted by the present invention is:
[0005] The first aspect of the present invention provides a method for treating transition metal wastewater, comprising the following steps:
[0006] Under light irradiation and power supply, a photocatalytic system including a photocatalytic anode is used to treat transition metal wastewater, and transition metals are deposited on the surface of the photocatalytic anode;
[0007] The photocatalytic anode comprises conductive glass loaded with titanium dioxide nanorod arrays.
[0008] Preferably, in the transition metal wastewater treatment method, the conductive glass includes at least one of FTO conductive glass and ITO conductive glass.
[0009] Preferably, in this transition metal wastewater treatment method, the loading amount of titanium element in the photocatalytic anode is 12-20 mg / cm 2 Further preferably, the loading amount of titanium element in the photocatalytic anode is 14-18 mg / cm 2 .
[0010] Preferably, in the transition metal wastewater treatment method, the transition metal wastewater contains at least one of free metal ions and / or complex metal ions of nickel, copper, manganese and cobalt.
[0011] In the present invention, a photocatalytic anode is used to generate photogenerated holes with strong oxidizing properties under light, and a transition metal such as manganese (Mn 2+ ) ions, nickel (Ni 2+ ) ions, cobalt (Co 2+ ) is oxidized to trivalent manganese (Mn 3+ ) or tetravalent manganese (Mn 4+ ), tetravalent nickel (Ni 4+ ), trivalent cobalt (Co 3+ ) or tetravalent cobalt (Co 4+ ) morphology, forming corresponding transition metal oxides and adsorbing on the surface of the photocatalytic anode, thereby achieving the selective removal of transition metals and the enrichment of transition metals on the anode surface.
[0012] Preferably, in the transition metal wastewater treatment method, the pH of the transition metal wastewater is 7-12; further preferably, the pH of the transition metal wastewater is 8-9.
[0013] Preferably, in this transition metal wastewater treatment method, the complexing agent to which the complexed metal ions are bound includes at least one of EDTA, phosphate, hydroxycarboxylate, and aminocarboxylate; further preferably, the complexing agent to which the complexed metal ions are bound is EDTA.
[0014] Preferably, in the transition metal wastewater treatment method, ultraviolet light is used for light irradiation; further preferably, weak ultraviolet light is used for light irradiation, and the wavelength of the weak ultraviolet light is 320nm-400nm.
[0015] Preferably, in this transition metal wastewater treatment method, direct current is used for power supply; the current density of the direct current is 0.2 mA / cm 2 -2.0mA / cm 2 If the current is too small, the decomposition effect of transition metal complexes in sewage is not obvious, and the transition metal removal effect is not good. If the current is too large, although a good decomposition effect can be achieved, it wastes power.
[0016] Preferably, in this transition metal wastewater treatment method, the electrolysis time is 120-200 minutes.
[0017] Preferably, in the transition metal wastewater treatment method, the preparation method of the photocatalytic anode comprises the following steps:
[0018] A titanium source solution and conductive glass are placed in a reaction container to carry out a hydrothermal reaction to obtain the photocatalytic anode.
[0019] Preferably, in the photocatalytic anode preparation method, the conductive glass is cleaned before the reaction; the cleaning solution can be ultrapure water, acetone, alcohol or a mixed solution of any combination thereof, and the ultrasonic cleaning time is 10-30 minutes.
[0020] Preferably, in this photocatalytic anode preparation method, the titanium source solution is a tetrabutyl titanate solution, and the concentration of the tetrabutyl titanate solution is 2-4 mol / L; further preferably, the concentration of the tetrabutyl titanate solution is 2.5-3.5 mol / L; further preferably, the concentration of the tetrabutyl titanate solution is 2.8-3.1 mol / L.
[0021] Preferably, in the method for preparing the photocatalytic anode, the hydrothermal reaction time is 4-6 h; further preferably, the hydrothermal reaction time is 4.5-5.5 h.
[0022] Preferably, in the method for preparing the photocatalytic anode, the temperature of the hydrothermal reaction is 500-600°C; further preferably, the temperature of the hydrothermal reaction is 520-580°C.
[0023] The second aspect of the present invention provides a transition metal recovery method, comprising the following steps: after the above-mentioned transition metal wastewater treatment method is used, a reverse current is applied or the photoanode is removed and placed in an acid solution to achieve the recovery of the transition metal.
[0024] The beneficial effects of the present invention are:
[0025] The transition metal wastewater treatment method of the present invention can be used for decomposing transition metal complexes. The decomposition process of the transition metal complexes of the present invention occurs in the anode chamber. When the photocatalytic anode is illuminated, photogenerated holes and active oxygen with strong oxidizing properties are generated to oxidize the transition metal complexes to separate organic groups from the transition metals, and the organic groups are converted into inorganic substances, thereby achieving the removal of the transition metal complexes and completing the deposition of the transition metals at the photoanode.
[0026] The present invention belongs to photoelectrocatalysis and can achieve the effect of saving electric energy; and the use of electric-assisted photocatalysis can reduce the hole recombination rate, strengthen the generation process of photogenerated holes, and improve the efficiency of transition metal ion treatment.
[0027] When the present invention performs high-concentration nickel ion removal or low-concentration continuous removal, nickel oxide directly detached from the anode surface can be obtained, and direct recovery can be achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 A diagram of a photocatalytic system device according to an embodiment.
[0029] Figure 2 This is a scanning electron microscope image of the photoanode of Example 1.
[0030] Figure 3 This is the photoanode energy spectrum analysis diagram of Example 1.
[0031] Figure 4 This is a trend chart of the Ni(II)-EDTA degradation rate in Example 2.
[0032] Attached Figure 1 mark:
[0033] 100 - first acrylic plate, 200 - first gasket, 300 - photoanode, 400 - second gasket, 500 - anode reaction chamber, 600 - third gasket, 700 - proton membrane, 800 - fourth gasket, 900 - cathode reaction chamber, 1000 - fifth gasket, 1100 - second acrylic plate. DETAILED DESCRIPTION
[0034] The present invention is further described in detail below by specific examples. Unless otherwise specified, the raw materials, reagents or devices used in the examples and comparative examples can be obtained from conventional commercial sources or can be obtained by prior art methods. Unless otherwise specified, the experiments or test methods are conventional methods in the art.
[0035] Use attached Figure 1 The photocatalytic system shown in the figure is used for transition metal wastewater treatment. Figure 1As shown, the entire reactor is assembled, sewage enters from the small hole above the anode reaction chamber 500, and sodium bicarbonate buffer is added to the cathode reaction chamber 900. At the same time, direct current and ultraviolet light are turned on according to the reaction conditions. During the reaction, continuous sampling is performed through the small hole above the anode reaction chamber 500. After the reaction is completed, the sewage after the reaction is taken out from the small hole above the anode reaction chamber 500 for relevant data detection.
[0036] Example 1
[0037] This embodiment provides a method for preparing a TiO2 nanorod array (photoanode) deposited on FTO, which specifically comprises the following steps:
[0038] The FTO conductive glass was ultrasonically cleaned in a mixed solution of ultrapure water, acetone and isopropanol (no requirement for solution concentration) for 20 minutes, and then the ultrasonically cleaned FTO conductive glass was placed in a mixed solution of hydrochloric acid, ultrapure water and tetrabutyl titanate (2.94 mol / L), and placed in a polytetrafluoroethylene pressure cooker, and then placed in a drying oven and set to a temperature of 550°C for hydrothermal reaction for 5 hours to obtain a FTO deposited TiO2 nanorod array photoanode.
[0039] SEM images of the photoanode are shown in Figure 2 As shown in the energy spectrum analysis diagram Figure 3 The photoanode prepared in this example is used in the following examples.
[0040] Example 2
[0041] A method for treating wastewater containing Ni(II)-EDTA, the specific process is as follows:
[0042] Use Figure 1 The photocatalytic system device shown uses an FTO-deposited TiO2 nanorod array as a photoanode, a platinum electrode as a cathode, and a 5ppm Ni-EDTA electrolyte. The photocatalytic anode is irradiated with 384nm ultraviolet light and supplemented with 2.8mA direct current. The solution pH is adjusted to 8.5 with sulfuric acid and sodium hydroxide. The electrolysis is performed for 150min. The Ni(Ⅱ)-EDTA degradation rate can reach 80%, and the cationic deposited nickel recovery rate can reach 40%.
[0043] The present invention conducts Ni 2+ Ion recovery occurs in the anode reaction chamber. When the device is working, since alkali metal, alkaline earth metal ions and iron ions cannot be photocatalytically oxidized, the deposition of alkali metal, alkaline earth metal ions and iron ions on the electrode can be avoided, achieving Ni 2+ Ion selective recovery.
[0044] The present invention utilizes the photocatalytic anode to generate photogenerated holes with strong oxidizing properties under the condition of light, and converts the divalent nickel (Ni 2+) ions are oxidized to trivalent nickel (Ni 3+ ) or tetravalent nickel (Ni 4+ ) morphology, forming corresponding nickel-containing oxides and adsorbing on the surface of the photocatalytic anode, thereby achieving the selective removal of metallic nickel and the enrichment of nickel on the anode surface.
[0045] Example 3
[0046] A method for treating wastewater containing Ni(II)-EDTA, the specific process is as follows:
[0047] Use Figure 1 The photocatalytic system device shown uses an FTO-deposited TiO2 nanorod array as a photoanode, a platinum electrode as a cathode, and a 5ppm Ni(Ⅱ)-EDTA electrolyte. The photocatalytic anode is irradiated with 384nm ultraviolet light and supplemented with 0mA direct current. The pH of the solution is adjusted to 8.5 with sulfuric acid and sodium hydroxide. The electrolysis is carried out for 150min, and the Ni(Ⅱ)-EDTA degradation rate can reach 10%.
[0048] Example 4
[0049] A method for treating wastewater containing Ni(II)-EDTA, the specific process is as follows:
[0050] Use Figure 1 The photocatalytic system device shown uses FTO deposited TiO2 nanorod array as the photoanode, a platinum electrode as the cathode, a 5ppm Ni(Ⅱ)-EDTA electrolyte, a direct current of 2.8mA, sulfuric acid and sodium hydroxide to adjust the solution pH to 8.5, electrolysis for 150min, the Ni(Ⅱ)-EDTA degradation rate is 30%, and the cationic deposited nickel recovery rate can reach 10%.
[0051] Example 5
[0052] A method for treating wastewater containing nickel ions, the specific process is:
[0053] Use Figure 1 The photocatalytic system device shown uses an FTO-deposited TiO2 nanorod array as a photoanode, a platinum electrode as a cathode, and a 10ppm nickel nitrate electrolyte. The photocatalytic anode is irradiated with 384nm ultraviolet light and supplemented with 2.1mA direct current. The solution pH is adjusted to 7 with sulfuric acid and sodium hydroxide. The electrolysis is performed for 120 minutes, and the nickel ion removal rate can reach 90%.
[0054] Example 6
[0055] A method for treating wastewater containing nickel ions, the specific process is:
[0056] Use Figure 1The photocatalytic system device shown uses an FTO-deposited TiO2 nanorod array as a photoanode, a platinum electrode as a cathode, and a 10ppm nickel nitrate electrolyte. The photocatalytic anode is irradiated with 384nm ultraviolet light and supplemented with 2.8mA direct current. The solution pH is adjusted to 7 with sulfuric acid and sodium hydroxide. The electrolysis is performed for 150min, and the nickel ion removal rate can reach 92%.
[0057] Example 7
[0058] A method for treating wastewater containing nickel ions, the specific process is:
[0059] Use Figure 1 The photocatalytic system device shown uses an FTO-deposited TiO2 nanorod array as a photoanode, a platinum electrode as a cathode, and a 10ppm nickel nitrate electrolyte. The photocatalytic anode is irradiated with 384nm ultraviolet light and supplemented with 1.4mA direct current. The solution pH is adjusted to 7 with sulfuric acid and sodium hydroxide. The electrolysis is performed for 150 minutes, and the nickel ion removal rate can reach 81%.
[0060] Example 8
[0061] A method for recovering nickel ions, the specific process is:
[0062] The nickel oxide attached to the above-mentioned Example 2 was used as a photocatalytic anode, a platinum electrode as a cathode, and sodium sulfate as an electrolyte. The photocatalytic anode was irradiated with 384nm ultraviolet light and supplemented with -1mA direct current. After 1 minute, all the nickel oxide attached to the titanium dioxide nanorod array photoanode electrolysis was released.
[0063] Example 9
[0064] A method for recovering nickel ions, the specific process is:
[0065] The titanium dioxide nanorod array photoanode with nickel oxide deposited after the reaction in Example 2 was placed in a reactor, and 0.1 M dilute sulfuric acid was added to react for 10 minutes, and all the nickel oxide attached to the titanium dioxide nanorod array photoanode was released and recovered after electrolysis.
[0066] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principles of the present invention shall be equivalent replacement modes and shall be included in the protection scope of the present invention.
Claims
1. A method for treating transition metal wastewater, characterized in that: The following steps are involved: Under light irradiation and power supply, a photocatalytic system including a photocatalytic anode is used to treat transition metal wastewater, and transition metals are deposited on the surface of the photocatalytic anode; The photocatalytic anode is a conductive glass loaded with titanium dioxide nanorod arrays; The conductive glass includes at least one of FTO conductive glass and ITO conductive glass; The titanium loading of the photocatalytic anode is 12-20 mg / cm 2 ; The transition metal wastewater contains at least one of free metal ions and / or complex metal ions of nickel; The complexing agent to which the complexed metal ions are bound includes at least one of EDTA, phosphate, hydroxycarboxylate and aminocarboxylate.
2. The transition metal wastewater treatment method according to claim 1, characterized in that: The pH of the transition metal wastewater is 7-12.
3. The transition metal wastewater treatment method according to claim 1, characterized in that: The light irradiation uses ultraviolet light.
4. The method for treating transition metal wastewater according to claim 1, characterized in that: The power supply adopts direct current; the current density of the direct current is 0.2mA / cm 2 -2.0mA / cm 2 .
5. The method for treating transition metal wastewater according to claim 1, characterized in that: The method for preparing the photocatalytic anode comprises the following steps: A titanium source solution and conductive glass are placed in a reaction container to carry out a hydrothermal reaction to obtain the photocatalytic anode.
6. The method for treating transition metal wastewater according to claim 5, characterized in that: The hydrothermal reaction time is 4-6h.
7. A transition metal recovery method, characterized in that: The method comprises the following steps: after the treatment by the transition metal wastewater treatment method according to any one of claims 1 to 6, applying a reverse current or taking out the photoanode and placing it in an acid solution to achieve the recovery of the transition metal.