A method for preparing tannin resin for adsorption and separation of nuclides and heavy metals

The preparation of tannin resin through hydrolysis and crosslinking processes solves the problem of difficult water solubility of tannins, realizes its effective application in nuclide adsorption and wastewater treatment, and provides high safety and environmentally friendly adsorption materials.

CN115850624BActive Publication Date: 2024-11-08SOUTHWEAT UNIV OF SCI & TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211581126.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-09
Publication Date
2024-11-08
Estimated Expiration
2042-12-09

AI Technical Summary

Technical Problem

Plant tannins have good water solubility and are difficult to recycle and directly utilize, which limits their application in nuclide adsorption materials.

Method used

After hydrolysis of alkaline water bath, adjust the pH and use aldehyde crosslinking agent to polymerize tannins intermolecular molecules to form an insoluble tannin resin. Combined with deionized water rinsing and drying processes, a process for adsorption and separation of nuclides and heavy metals was prepared. Tannin resin.

Benefits of technology

The highly solubility tannins are successfully converted into insoluble tannins resin, retaining their adsorption properties, and solving the utilization problems in wastewater treatment, providing high safety and environmentally friendly adsorption materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115850624B_ABST
    Figure CN115850624B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a tannin resin for adsorption and separation of nuclides and heavy metals, comprising: preparing a tannin solution, hydrolyzing it in an alkali water bath to obtain a tannin solution with a small molecular weight; adjusting the pH of the tannin solution after the water bath hydrolysis to be acidic, and polymerizing the tannin molecules with each other under heating conditions through the action of an aldehyde cross-linking agent to form a tannin resin crude material; washing the tannin resin crude material with deionized water to remove unreacted aldehydes and tannins, and then drying to obtain the tannin resin. The invention effectively solves the problem of the reuse of tannin biomass resources and the problem that tannin cannot be directly used in wastewater treatment due to its good solubility. The tannin resin prepared by the invention can achieve a good adsorption and separation effect on uranyl ions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparation of pollution adsorption materials, and more specifically, relates to a method for preparing tannin resin for adsorption and separation of nuclides and heavy metals. Background Art

[0002] Plant tannins, also known as plant polyphenols, have a relative molecular weight in the range of 500 to 3000. They are a mixture of phenolic compounds that can react with proteins, alkaloids and gelatin to precipitate. They are different from alkaloids because they do not contain nitrogen. They are one of the secondary metabolites in plants. They are widely distributed in the skin, wood, leaves, roots, fruits and other parts of plants. In particular, the tannin content in galls can reach 50% to 70%. Western my country is rich in plant tannin resources. The tannin content of some plants can reach 20% to 30%, and high-quality varieties can even exceed 40%. For example, the tannin content in gallnut is about 70%. The structure of plant tannins is generally a benzene ring with o-dihydroxy or o-trihydroxy, which is usually divided into two categories: hydrolyzed tannins and condensed tannins. Hydrolyzed tannins are formed by phenolic acid and hydroxyl groups through glycosidic bonds or lipid bonds. They are easily hydrolyzed by acids or enzymes. According to the different hydrolysis products, they can be divided into gallotannins and ellagic tannins. The product of gallotannins is gallic acid, and the products of ellagic tannins are hexahydroxydiphenic acid and ellagic acid. They are mainly derived from plants such as nuts, chestnuts, oaks, and pomegranate barks. Condensed tannins, also known as procyanidins, are formed by condensation of hydroxyflavanoid compounds with carbon-carbon bonds. Unlike hydrolyzed tannins, they can be polymerized or decomposed into water-insoluble reddish-brown compounds under the action of acids and enzymes. They are mainly derived from vegetables and fruits, such as catechins in tea, grape tannins, and persimmon tannins. Research has found that tannins have antioxidant, antiviral, antibacterial, anti-radiation, and anti-ultraviolet activities, and have been used in various fields such as food packaging, winemaking, medicine, beauty, textiles, and animal husbandry.

[0003] The complexation reaction between the phenolic hydroxyl groups in tannin and metal ions is one of the characteristic reactions of tannin. In the tannin solution, the tannin molecules have a certain ionization equilibrium. The phenolic hydroxyl groups in the tannin molecules can ionize hydrogen ions, and the remaining oxygen anions can react stably with metal ions. The phenolic hydroxyl groups that have not been ionized can also react with metal ions, but the stability is relatively poor.

[0004] Tannin is highly water-soluble and difficult to recycle, so it cannot be directly used as an adsorption material for metal ions in industry. By using formaldehyde to cross-link and polymerize tannin molecules to generate insoluble tannin resin, tannin can be used for radionuclide adsorption. Summary of the invention

[0005] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.

[0006] In order to achieve these purposes and other advantages according to the present invention, a method for preparing a tannin resin for the adsorption and separation of nuclides and heavy metals is provided, comprising the following steps:

[0007] Step 1, preparing a tannin solution, and hydrolyzing it in an alkaline water bath to obtain a tannin solution with a small molecular weight;

[0008] Step 2: adjusting the pH of the tannin solution after water bath hydrolysis to acidic, and polymerizing the tannin molecules with each other through the action of aldehyde cross-linking agent under heating conditions to form a tannin resin crude material;

[0009] Step 3: Rinse the tannin resin crude material with deionized water to remove unreacted aldehyde and tannin, and then dry to obtain tannin resin.

[0010] Preferably, in the step 1, the tannin is bayberry tannin.

[0011] Preferably, the aldehyde cross-linking agent is formaldehyde.

[0012] Preferably, in step one, the specific process steps for preparing the tannin solution include: dissolving bayberry tannin in deionized water, wherein the mass volume ratio of bayberry tannin to deionized water is 1 g:10 mL.

[0013] Preferably, in the step 1, a low molecular weight tannin solution is obtained by hydrolysis in an alkaline water bath, and the specific process steps include: dissolving bayberry tannin in deionized water, adding 30% by mass NaOH solution and 30% by mass H 2 O 2 The solution was heated in a water bath at 60 °C for 2 h, wherein tannin, deionized water, NaOH solution and H 2 O 2 The mass volume ratio of the solution is 10g:100mL:4mL:3mL.

[0014] Preferably, in the step 2, the pH of the tannin solution is adjusted to be acidic, and the tannin molecules are polymerized with each other through the action of aldehyde cross-linking agents under heating conditions to form a tannin resin crude material. The specific process steps are as follows: the pH of the bayberry tannin solution is adjusted to 1 with concentrated hydrochloric acid, formaldehyde solution is added, and then heated in a water bath at 90°C with stirring for 2 hours, wherein the mass volume ratio of tannin to formaldehyde solution is 5g:1mL.

[0015] Preferably, in step three, the material is rinsed with deionized water to remove unreacted aldehyde and tannin, and then dried to obtain the tannin resin. The specific process steps are: washing with deionized water three times, removing moisture from the material with a suction filter, and then placing it in an oven and drying it at 45°C for 24 hours.

[0016] Preferably, in the step 3, the dried tannin resin is ground to obtain Al 2 O 3 As grinding media, Al 2 O 3 The mass ratio of cerium hydroxide to tannin resin is 3 to 5:1, the tannin resin is ground into powder with an average particle size of 5 to 200 μm, and the powder is sieved after grinding. The sieved tannin resin powder is added into a cerium hydroxide suspension, the mass ratio of the solid content of cerium hydroxide in the cerium hydroxide suspension to the tannin resin powder is 1:25, and after stirring evenly, centrifuging at a speed of 2500 to 3000 r / min to obtain a mixed precipitate of cerium hydroxide and tannin resin, and filtering out the mixed precipitate to obtain tannin resin doped with cerium hydroxide.

[0017] The present invention at least includes the following beneficial effects: In view of the problem that tannin is very water-soluble and difficult to be directly utilized, the present invention provides a method for preparing tannin resin for adsorption and separation of nuclides and heavy metals. The tannin resin prepared by the preparation method provided by the present invention effectively solves the problem of recycling tannin biomass resources and the problem that tannin is too soluble and cannot be directly utilized in wastewater treatment. Bayberry tannin is a complex phenolic substance with a benzene ring as the basic skeleton, containing a large number of phenolic hydroxyl groups. The presence of phenolic hydroxyl groups on the A ring of bayberry tannin increases the activity of ortho-hydrogen and para-hydrogen, providing a binding site for the polymerization of phenolic resin. The two highly nucleophilic active sites of the A ring in the structural unit of bayberry tannin react with formaldehyde, so that cross-linking polymerization occurs between bayberry tannins, thereby obtaining tannin resin. The obtained tannin resin has the characteristics of high safety and environmental friendliness, and can be applied to industrial wastewater treatment, heavy metal extraction, daily chemicals, environment and other fields. The present application utilizes the principle that tannin and formaldehyde undergo polycondensation to form tannin resin, so that highly soluble tannin is synthesized into insoluble tannin resin, which not only retains the adsorption performance of tannin to radionuclides, but also enables tannin to be utilized in practical problems such as wastewater treatment.

[0018] Plant tannins are abundant in nature and are a renewable, green and environmentally friendly natural resource with broad application prospects. This application utilizes this abundant natural biomass material, and the tannin resin obtained exhibits good adsorption performance, and has the advantages of high safety and environmental protection. The synthesis of tannin resins has broadened the scope of application of plant tannins. In an era of rapid development of industrialization, it is particularly important to implement the concept of sustainable development and the development and utilization of highly safe and environmentally friendly materials. Making full use of the ability of natural biomass resources, plant tannins, to adsorb radionuclides to develop environmentally friendly materials is a route that conforms to contemporary themes.

[0019] The bayberry tannin phenolic resin material obtained by the present invention can be used for treating wastewater containing heavy metal ions, and can be used for treating uranyl ions (UO 2 2+ ) has good adsorption effect and is an environmentally friendly adsorbent with low economic cost and broad application prospects.

[0020] Adding cerium hydroxide in an amount of 1 / 25 of the mass of the bayberry tannin phenolic resin into the subsequently prepared bayberry tannin phenolic resin has a greater adsorption capacity for uranyl ions.

[0021] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The schematic diagram of the synthesis route for preparing the tannin resin in Example 1 is shown;

[0023] Figure 2 This is the infrared spectrum of the tannin resin prepared in Example 1 before and after the adsorption of potassium bromide and the red bayberry tannin as a control;

[0024] Figure 3 The tannin resin prepared in Example 1 adsorbs UO 2 2+ Local SEM image before;

[0025] Figure 4 The tannin resin prepared in Example 1 adsorbs UO 2 2+ Local SEM image before;

[0026] Figure 5 The tannin resin prepared in Example 1 adsorbs UO 2 2+ Local SEM image before;

[0027] Figure 6 The tannin resin prepared in Example 1 adsorbs UO2 2+ The local scanning electron microscope image after

[0028] Figure 7 The tannin resin prepared in Example 1 adsorbs UO 2 2+ The local scanning electron microscope image after

[0029] Figure 8 The tannin resin prepared in Example 1 adsorbs UO 2 2+ The local scanning electron microscope image after

[0030] Fig. 9 This is the C element spectrum of the tannin resin prepared in Example 1;

[0031] Fig.10 This is the O element spectrum of the tannin resin prepared in Example 1;

[0032] Fig.11 This is the U element spectrum of the tannin resin prepared in Example 1;

[0033] Fig.12 This is a scanning electron microscope image of bayberry tannin resin;

[0034] Fig.13 The results of the preparation of the bayberry tannin resin in Example 1 on the effect of UO under different pH conditions 2 2+ Schematic diagram of adsorption capacity;

[0035] Fig.14 The different dosages of the bayberry tannin resin prepared in Example 1 were used to treat UO 2 2+ Schematic diagram of adsorption capacity;

[0036] Fig.15 The different adsorption times of the bayberry tannin resin prepared in Example 1 on UO 2 2+ Schematic diagram of adsorption capacity;

[0037] Fig.16 The waxberry tannin resin prepared in Example 1 and the waxberry tannin resin doped with cerium hydroxide prepared in Example 2 were not subjected to adsorption time for UO 2 2+ Schematic diagram of adsorption capacity comparison. DETAILED DESCRIPTION

[0038] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.

[0039] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.

[0040] Example 1

[0041] This embodiment provides a method for preparing a tannin resin for the adsorption and separation of nuclides and heavy metals, comprising the following steps:

[0042] Step 1: prepare bayberry tannin solution, the specific steps include: taking 100g bayberry tannin and adding it to 1000mL deionized water, adding 40mL 30% NaOH solution and 30mL 30% H 2 O 2 The solution was stirred in a water bath at 60°C for 2 h to obtain a hydrolyzed bayberry tannin solution.

[0043] Step 2: Use 6M HCl to adjust the pH of the bayberry tannin solution to 1.0, add 20mL of formaldehyde, and stir in a 90°C water bath for 2h to use formaldehyde to cause a cross-linking reaction between bayberry tannin molecules. After the reaction is completed, rinse the residual formaldehyde and bayberry tannin with deionized water to obtain the product tannin resin.

[0044] Step 3: Place the obtained tannin resin in an oven and bake at 45° C. for 24 hours. After drying, crush it with a grinder to obtain the final product.

[0045] The preparation synthesis route of the bayberry tannin resin in Example 1 is drawn as follows: Figure 1 shown.

[0046] Example 2

[0047] Take 500g of the bayberry tannin resin prepared in Example 1, grind it, and add 1500g of Al 2 O 3 The method comprises the following steps: grinding the bayberry tannin resin into a powder with an average particle size of 5 μm using 200 μm as a grinding medium, sieving the powder after grinding, adding the sifted bayberry tannin resin powder into a cerium hydroxide suspension, wherein the solid content of cerium hydroxide in the cerium hydroxide suspension is 20 g, stirring evenly, centrifuging at a speed of 2500 r / min to obtain a mixed precipitate of cerium hydroxide and bayberry tannin resin, filtering the mixed precipitate to obtain bayberry tannin resin doped with cerium hydroxide.

[0048] Taking bayberry tannin (referred to as BT) as a control, the tannin resin (referred to as BT-PR-NSs) prepared in Example 1 was weighed and the mixture was ground with potassium bromide at a mass ratio of 1:10 under an infrared lamp, and the mixture was pressed into a tablet using a tablet press. The prepared flakes were placed at 4000-400 cm -1Fourier transform infrared spectroscopy (FT-IR, PerkinElmer, USA) was performed to obtain infrared spectral data of BT and BT-PR-NSs before adsorption and infrared spectral data of BT-PR-NSs-U after adsorption. The results are as follows: Figure 2 shown.

[0049] From the Fourier infrared spectrum, we can see that bayberry tannin 3410cm -1 The hydroxyl absorption peak at 1717 cm-1 shifted after polymerization because the number of hydroxyl groups decreased after BT hydrolysis. -1 An obvious absorption peak appeared, which was due to the stretching vibration of the carbonyl bonds formed during the polymerization of bayberry tannin molecules, proving the successful polymerization of tannin resin.

[0050] Take 10mg of bayberry tannin and 10mg of adsorbed UO 2 2+ The BT-PR-NSs adsorbent was observed under a scanning electron microscope. Figure 3-Figure 8 As shown, Figure 3-Figure 5 To adsorb UO 2 2+ Scanning electron microscopy image of BT-PR-NSs adsorbent before Figure 6-Figure 8 To adsorb UO 2 2+ The scanning electron microscope image of the BT-PR-NSs adsorbent after polymerization shows that the morphology of the BT and BT-PR-NSs adsorbents before and after polymerization has changed. This is because the hydrolysis process destroys the original molecular morphology of bayberry tannins, which is the result of repolymerization. 2 2+ Energy spectrum analysis was done before and after, and the results are as follows Figure 9-11 As shown, Fig. 9 , Fig.10 and Fig.11 The energy spectra of C, O, and U are shown respectively. The results show that the surface BT-PR-NSs adsorbent is composed of C and O elements. 2 2+ After adsorption, the U element is evenly distributed on the surface of the adsorbent, indicating that the BT-PR-NSs adsorbent is suitable for UO 2 2+ It has good adsorption effect. The scanning electron microscope image of bayberry tannin resin is as follows Fig.12 shown.

[0051] In order to verify the adsorption of BT-PR-NSs on UO 2 2+ The adsorption performance of the adsorbent under different pH environments was investigated.2 2+ The solution was adjusted to pH 2, 3, 4, 5, and 6 respectively, and UO 2 2+ 50 mL of the solution was placed in a 150 mL conical flask, and 15 mg of BT-PR-NSs adsorbent was placed in the conical flask. The constant temperature oscillation box was set to 25 °C and the speed was 150 r / min. The conical flask was placed in the constant temperature oscillation for 24 h. After 24 h, the residual UO was determined using an enzyme marker. 2 2+ concentration, and calculated the adsorption capacity of BT-PR-NSs adsorbent. The results are as follows Fig.13 .

[0052] In order to verify the adsorption of BT-PR-NSs on UO 2 2+ The adsorption performance of different adsorbent dosages was investigated. 2 2+ Solution, adjust pH to 5, take UO 2 2+ 50 mL of the solution was placed in a 150 mL conical flask, and 10 mg, 15 mg, 20 mg, 25 mg, and 30 mg of BT-PR-NSs adsorbent were taken into the conical flask respectively. The constant temperature oscillation box was set at 25 °C and the speed was 150 r / min. The conical flask was placed in the constant temperature oscillation for 24 h. After 24 h, the residual UO was determined using an enzyme marker 2 2+ concentration, and calculated the adsorption capacity of BT-PR-NSs adsorbent. The results are as follows Fig.14 , Fig.14 The horizontal axis in the figure is the dosage of BT-PR-NSs adsorbent, the vertical axis on the left is the adsorption capacity (mg / g), and the vertical axis on the right is the UO 2 2+ The removal rate of UO is shown in Figure 2. Line segment a represents the effect of different adsorbent dosages on the removal rate of UO. 2 2+ The line segment b represents the change of adsorption capacity of UO with different adsorbent dosages. 2 2+ removal rate.

[0053] In order to verify the adsorption of BT-PR-NSs on UO 2 2+ The adsorption performance of different adsorption times was investigated. 2 2+ Solution, adjust pH to 5, take UO 2 2+50 mL of the solution was placed in a 150 mL conical flask, 15 mg of BT-PR-NSs adsorbent was taken and placed in the conical flask, the constant temperature oscillation box was set to 25 °C and the speed was 150 r / min, the conical flask was placed in the constant temperature oscillation for 2 min, 4 min, 6 min, 8 min, 10 min, 20 min, 30 min, 60 min, 120 min, 180 min, 240 min, 360 min, 480 min, and the residual UO was determined using an enzyme marker 2 2+ concentration, and calculated the adsorption capacity of BT-PR-NSs adsorbent. The results are as follows Fig.15 .

[0054] Comparative Example 1 prepared bayberry tannin resin and Example 2 prepared bayberry tannin resin doped with cerium hydroxide on UO at different times 2 2+ The adsorption capacity change is Fig.16 ;from Fig.16 It can be seen that the bayberry tannin doped with cerium hydroxide prepared in Example 2 has a greater adsorption capacity for uranyl ions.

[0055] The number of devices and processing scales described here are used to simplify the description of the present invention. Applications, modifications and variations of the present invention will be obvious to those skilled in the art.

[0056] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.

Claims

1. A method for preparing tannin resin for adsorption and separation of nuclides and heavy metals, It is characterized in that The following steps are involved: Step 1, preparing a tannin solution, and hydrolyzing it in an alkaline water bath to obtain a tannin solution with a small molecular weight; Step 2: adjusting the pH of the tannin solution after water bath hydrolysis to acidic, and polymerizing the tannin molecules with each other through the action of aldehyde cross-linking agent under heating conditions to form a tannin resin crude material; Step 3: Rinse the tannin resin crude material with deionized water to remove unreacted aldehyde and tannin, and then dry to obtain tannin resin; In the step 1, the tannin is bayberry tannin; In the step 2, the pH of the tannin solution is adjusted to be acidic, and the tannin molecules are polymerized with each other through the action of an aldehyde cross-linking agent under heating conditions to form a tannin resin crude material. The specific process steps are as follows: the pH of the bayberry tannin solution is adjusted to 1 with concentrated hydrochloric acid, a formaldehyde solution is added, and then heated in a water bath at 90° C. with stirring for 2 hours, wherein the mass volume ratio of the tannin to the formaldehyde solution is 5 g:1 mL; In the step 3, the dried tannin resin is ground to obtain Al 2 O 3 As grinding media, Al 2 O 3 The mass ratio of cerium hydroxide to tannin resin is 3 to 5:1, the tannin resin is ground into powder with an average particle size of 5 to 200 μm, and the powder is sieved after grinding. The sieved tannin resin powder is added into a cerium hydroxide suspension, the mass ratio of the solid content of cerium hydroxide in the cerium hydroxide suspension to the tannin resin powder is 1:25, and after stirring evenly, centrifuging at a speed of 2500 to 3000 r / min to obtain a mixed precipitate of cerium hydroxide and tannin resin, and filtering out the mixed precipitate to obtain tannin resin doped with cerium hydroxide.

2. The method for preparing the tannin resin for the adsorption and separation of nuclides and heavy metals according to claim 1, It is characterized in that The aldehyde cross-linking agent is formaldehyde.

3. The method for preparing the tannin resin for the adsorption and separation of nuclides and heavy metals according to claim 1, It is characterized in that In the step 1, the specific process steps for preparing the tannin solution include: dissolving bayberry tannin in deionized water, wherein the mass volume ratio of bayberry tannin to deionized water is 1 g:10 mL.

4. The method for preparing the tannin resin for the adsorption and separation of nuclides and heavy metals as claimed in claim 1, It is characterized in that In the step 1, a low molecular weight tannin solution is obtained by hydrolysis in an alkaline water bath. The specific process steps include: dissolving bayberry tannin in deionized water, adding 30% by mass NaOH solution and 30% by mass H 2 O 2 The solution was heated in a water bath at 60 °C for 2 h, wherein tannin, deionized water, NaOH solution and H 2 O 2 The mass volume ratio of the solution is 10g:100mL:4mL:3mL.

5. The method for preparing the tannin resin for the adsorption and separation of nuclides and heavy metals as claimed in claim 1, It is characterized in that In the step three, the tannin resin is obtained by rinsing with deionized water to remove unreacted aldehyde and tannin, and then drying. The specific process steps are: washing with deionized water three times, removing moisture from the material with a suction filter, and then placing it in an oven and drying it at 45° C. for 24 hours.