Halogen-free flame-retardant polyamide elastomer material and preparation method and application thereof
By using aluminum hypophosphate and zinc borate as flame retardant in polyamide elastomers, combined with coupling agent and dispersant, a high-compatibility flame retardant system is formed, and the mechanical properties and hydrolysis resistance of halogen-free flame retardant materials are solved. The problem of this achieves efficient flame retardant and environmentally friendly halogen-free and low smoke effects.
Patent Information
- Application Number
- CN202211511519.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-29
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-11-29
AI Technical Summary
While the existing halogen-free flame-retardant polyamide elastomer materials achieve flame retardant properties, their mechanical properties and hydrolysis resistance are insufficient, making it difficult to meet the use requirements of certain environments.
Aluminum hypophosphate and zinc borate are used as main synergistic flame retardants, combined with polyamide elastomer, and through the surface modification of coupling agent and the use of dispersant, a high-compatibility flame retardant system is formed, and melt-kneading and extrusion are carried out. Processing technology to prepare halogen-free flame-retardant polyamide elastomer materials.
The good flame retardant properties, mechanical properties and hydrolysis resistance of halogen-free flame retardant polyamide elastomer materials have been improved, and the flame retardant effect at V0 level has been achieved. The tensile strength and impact strength have been significantly improved, while maintaining the environmental protection of the material and Low smoke characteristics.
Smart Images

Figure BDA0003969276420000041 
Figure BDA0003969276420000141 
Figure BDA0003969276420000151
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyamide composite materials, and in particular to a halogen-free flame-retardant polyamide elastomer material and a preparation method and application thereof. Background Art
[0002] The flame retardant method generally used for flame retardant materials is to add flame retardants to the materials. Among them, halogenated and metal oxide flame retardants containing halogen have high flame retardant efficiency, but because these materials contain halides, they release a large amount of smoke and hydrogen halide gas when burning, which is not only toxic, but also greatly hinders safe evacuation and fire fighting. In addition, once the hydrogen halide gas reacts with water in the air, "hydrogen halide acid" is generated, which seriously corrodes instruments and equipment and buildings. Other halogen-free flame retardant materials, although they do not produce harmful gases and a large amount of smoke when burning, and do not corrode instruments and equipment, but due to the large amount of halogen-free flame retardants, the mechanical properties and electrical properties of the materials are reduced, and they have gradually been unable to meet the development and use needs of flame retardant materials. How to achieve green and environmentally friendly flame retardant materials and good mechanical properties while meeting the flame retardant requirements is a problem that needs to be solved.
[0003] Polyamide elastomer (TPAE), also known as thermoplastic polyamide elastomer, is a block copolymer containing polyamide hard segment and aliphatic polyester or polyether soft segment. It has the characteristics of low hardness, good flexibility, high tensile strength, good elastic recovery, high low-temperature impact strength, excellent low-temperature resistance, etc. It is easy to process and is very suitable for use in some fields that require high-strength and low-modulus elastomers. However, polyamide elastomers also have the disadvantages of low oxygen index and easy combustion. In some scenarios and products that need to be flame-retardant, such as halogen-free low-smoke flame-retardant cables, flame-retardant injection molded parts, etc., there are many restrictions. Therefore, the development of halogen-free flame-retardant polyamide elastomer materials is imminent.
[0004] There is little research on halogen-free flame-retardant polyamide elastomer materials on the market, and most of the flame-retardant elastomer materials are made by adding or blending organic and inorganic flame retardants. While achieving flame retardant properties, they are not resistant to hydrolysis, and the mechanical properties are greatly reduced, making it difficult to meet the use requirements of certain environments. Flame retardants make the material less flexible and have a higher hardness, while the flame retardant materials modified by elastomers have reduced tensile strength and impact properties.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] One of the purposes of the present invention is to provide a halogen-free flame-retardant polyamide elastomer material, which is a halogen-free flame-retardant elastomer material with excellent flame retardancy, good hydrolysis resistance and better mechanical properties.
[0007] The second object of the present invention is to provide a method for preparing the halogen-free flame-retardant polyamide elastomer material.
[0008] The third object of the present invention is to provide an application of the halogen-free flame-retardant polyamide elastomer material.
[0009] On one hand, the present invention provides a halogen-free flame-retardant polyamide elastomer material, which comprises the following components based on 100 parts by total weight: 55-75 parts of polyamide elastomer, 15-25 parts of main flame retardant, 3-15 parts of synergistic flame retardant, 0.4-2 parts of coupling agent, 0.5-3 parts of dispersant, 3-10 parts of compatibilizer, 0.1-1 parts of antioxidant, and 0.1-2 parts of absorbent;
[0010] The main flame retardant is at least one selected from red phosphorus, aluminum hypophosphite (AHP), diethyl aluminum hypophosphite (ADP), iso-tert-butyl aluminum hypophosphite (A-MBPa), ammonium polyphosphate (APP), disodium hydrogen phosphate, magnesium dihydrogen phosphate, lithium phosphate, magnesium phosphate, sodium phosphate, diammonium hydrogen phosphate and antimony phosphate, preferably aluminum hypophosphite (AHP);
[0011] The synergistic flame retardant is at least one selected from zinc borate (ZB), organic montmorillonite (OMMT), nanoclay, antimony trioxide, triphenylphosphonate (TPP), tricresyl phosphate (TCP), bisphenol A bis(diphenyl phosphate) (BDP), and resorcinol diphosphonate, preferably zinc borate (ZB).
[0012] For example, the halogen-free flame retardant polyamide elastomer material according to the embodiment of the present invention includes the following components based on 100 parts by total weight: 60-65 parts of polyamide elastomer, such as 62-65 parts; 20-25 parts of main flame retardant, such as 20-23 parts; 8-10 parts of synergistic flame retardant, such as 8-9 parts; 0.4-0.6 parts of coupling agent, such as 0.5-0.6 parts; 1-2 parts of dispersant, such as 1-2 parts; 3-10 parts of compatibilizer, such as 5-6 parts; 0.3-0.6 parts of antioxidant, such as 0.3-0.5 parts; 0.3-0.5 parts of absorbent, such as 0.3-0.4 parts.
[0013] For another example, the halogen-free flame retardant polyamide elastomer material of one embodiment of the present invention includes the following components based on 100 parts by total weight: 62-65 parts of polyamide elastomer, 22-23 parts of main flame retardant, 8-9 parts of synergistic flame retardant, 0.5-0.6 parts of coupling agent, 1-2 parts of dispersant, 5-6 parts of compatibilizer, 0.3-0.5 parts of antioxidant, and 0.3-0.4 parts of absorbent.
[0014] In the components of the halogen-free flame-retardant polyamide elastomer material of one embodiment of the present invention, the weight ratio of aluminum hypophosphite to zinc borate is 2-3:1, and the total weight of aluminum hypophosphite and zinc borate accounts for 25%-35% of the total weight of the halogen-free flame-retardant polyamide elastomer material.
[0015] Each component is described in detail below.
[0016] Polyamide elastomer
[0017] The polyamide elastomer resin is used as a flame retardant material substrate, has good flexibility and excellent mechanical properties. The polyamide elastomer can be a blend of one or more of long-chain or short-chain polyether block amide (PEBA), polyether ester amide (PEEA) and polyester amide (PEA) block copolymers. Considering the material performance and economy, it is preferably a polyether block amide, and more preferably a nylon 6 type polyether block polyamide elastomer (i.e., polyamide 6 type thermoplastic elastomer, TPAE-6).
[0018] In order to take into account both the processing flowability and mechanical properties of the composite material, the relative viscosity of the polyamide elastomer is preferably 1.5-3.0, preferably 2.0-2.8, and the hardness is preferably 45-60D. The relative viscosity is measured by the GB / T 12006.1 (ISO307) standard method with formic acid solution as solvent. The hardness is measured by the GB / T2411-2008 standard method.
[0019] In a preferred embodiment, a polyamide 6 type thermoplastic elastomer is prepared by a method (diacid) comprising the following steps: adding polyether / polyester, caprolactam, deionized water, a catalyst, and a diacid into a reactor, heating to 200-240° C. under nitrogen protection, and reacting for 0.5-2 hours under mechanical stirring; then evacuating to 20-500 Pa at 250-280° C. and continuing the mechanical stirring reaction for 0.5-3 hours; then extracting with boiling water and drying to obtain a polyamide 6 thermoplastic elastomer resin, wherein the diacid is oxalic acid, malonic acid, succinic acid or adipic acid, and wherein the catalyst is phosphoric acid, sulfuric acid, or aminocaproic acid.
[0020] Preferably, the polyether / polyester is one or more selected from polytetrahydrofuran, polyethylene glycol, polypropylene glycol and polyethylene glycol. Preferably, the number average molecular weight of the polyether / polyester is 300-8000. Preferably, based on the total weight of the polyether / polyester and caprolactam, the amount of the polyester / polyether is 10wt-60wt%. Preferably, based on the total weight of the polyether / polyester and caprolactam, the amount of the caprolactam is 40wt-90wt%; and / or the amount of the diacid is 1-10wt%; and / or the amount of the catalyst is 0.1-4wt%; and / or the amount of the deionized water is 0.5-4wt%. Preferably, the mechanical stirring speed is 100-800rpm.
[0021] In a preferred embodiment, the polyamide 6 type thermoplastic elastomer is prepared by the method disclosed in CN 104327266 B, the disclosure of which is fully incorporated herein by reference.
[0022] The relative viscosity of TPAE-6 prepared by this method is between 1.5 and 3.0 (measured by GB / T 12006.1 (ISO307) standard method with formic acid solution as solvent). TPAE-6 with stable viscosity can be obtained by more precise adjustment of reaction temperature and time.
[0023] The TPAE6 material preferably manufactured by the above-mentioned dibasic acid method has strong polarity, contains a large number of terminal amino groups and terminal carboxyl groups, has a short carbon chain, a relatively high N content, and has better flame retardant properties. It can be well combined with flame retardants and coupling agents to enhance the reaction compatibility of the composition system. At the same time, it can form strong hydrogen bonds with the flame retardant material molecules, thereby greatly improving the mechanical properties and flame retardant properties of the prepared flame retardant material.
[0024] Based on about 100 parts by weight of the halogen-free flame retardant polyamide elastomer material, the halogen-free flame retardant polyamide elastomer material may include about 55 parts by weight to about 75 parts by weight of the polyamide elastomer, for example, 55 parts by weight, 60 parts by weight, 65 parts by weight, 70 parts by weight, or 75 parts by weight.
[0025] Main flame retardant
[0026] The main flame retardant is a mixture of one or more selected from red phosphorus, aluminum hypophosphite (AHP), diethyl aluminum hypophosphite (ADP), iso-tert-butyl aluminum hypophosphite (A-MBPa), ammonium polyphosphate (APP), disodium hydrogen phosphate, lithium phosphate, magnesium phosphate, sodium phosphate, diammonium hydrogen phosphate and antimony phosphate, etc. Among them, the flame retardant effect of the combination of red phosphorus and polyamide elastomer is the best, and the effect is very good in non-natural color flame retardant materials, but considering the color pollution problem caused by red phosphorus and economic benefits, aluminum hypophosphite is preferred.
[0027] Aluminum hypophosphite has the characteristics of both aluminum hydroxide and hypophosphorous acid in structure, and its phosphorus content is very high. The structure is as follows:
[0028]
[0029] Aluminum hypophosphite flame retardant decomposes under heat and produces free radicals in the gas phase. These free radicals can capture high-energy free radicals in the flame area and convert them into stable free radicals, thereby inhibiting the radical-free radical chain reaction. In addition, in the condensed phase, aluminum hypophosphite will decompose into non-combustible solids, covering the surface of the burning object and isolating it from the air. At the same time, the Al 3+ It will react with POO-, thus promoting a series of reactions such as heat absorption, dehydration, and carbonization of the polymer, and finally forming a dense carbon layer. The carbon layer blocks the transfer of oxygen and heat in the condensed phase. This carbon layer is flame-retardant, heat-insulating, and oxygen-insulating, blocking the further decomposition of the bottom layer, thereby achieving a flame retardant effect. The water vapor generated by the reaction can also dilute the concentration of combustibles in the gas phase while reducing the condensed phase temperature, thereby better playing a flame retardant role.
[0030] In some embodiments, the particle size D90 of the aluminum hypophosphite is 2-5 μm. The particle size of the aluminum hypophosphite is moderate. If the particle size is too large, the performance of the elastomer material will be greatly damaged. If the particle size is too small, the cost will be high, and it will be easy to agglomerate and difficult to disperse. It is preferably 2 to 5 microns, and the particle size distribution should be as narrow as possible so as not to affect the stability of the material performance.
[0031] In some embodiments, the thermal weight loss temperature of the aluminum hypophosphite needs to be greater than 300°C (GB T 33047.1-2016), and the material processing temperature is preferably not higher than 280°C.
[0032] Based on about 100 parts by weight of the halogen-free flame retardant polyamide elastomer material, the halogen-free flame retardant polyamide elastomer material may include about 15 parts by weight to about 25 parts by weight of the main flame retardant, for example, 15 parts by weight, 20 parts by weight, or 25 parts by weight.
[0033] Synergistic flame retardants
[0034] The synergistic flame retardant is a mixture of one or more selected from zinc borate (ZB), organic montmorillonite (OMMT), nanoclay, antimony trioxide, triphenylphosphonate (TPP), tricresol phosphate (TCP), bisphenol A bis (diphenyl phosphate) (BDP), resorcinol diphosphonate, etc., preferably zinc borate (ZB), especially 3.5-hydrate zinc borate, with a particle size of 1-3 microns. When zinc borate is heated above 300°C, it decomposes to release crystal water, which plays the role of heat absorption, cooling and diluting oxygen. At the same time, the decomposed B2O3 forms a covering layer on the surface of the polymer, which cooperates with the carbon layer formed by aluminum hypophosphite to isolate air and heat, and has a flame retardant effect.
[0035] Based on about 100 parts by weight of the halogen-free flame retardant polyamide elastomer material, the halogen-free flame retardant polyamide elastomer material may include about 3 parts by weight to about 15 parts by weight of a synergistic flame retardant, for example, 3 parts by weight, 4 parts by weight, 5 parts by weight, 6 parts by weight, 7 parts by weight, 8 parts by weight, 9 parts by weight, 10 parts by weight, 12 parts by weight, 14 parts by weight, or 15 parts by weight.
[0036] Coupling agent
[0037] Coupling agents are used to modify the surface of flame retardants.
[0038] The coupling agent can be one or more of silane coupling agents such as KH560, KH550, KH570, KH792, DL602, etc., titanate coupling agents 201, 101, 105, 311, TTS, etc., preferably silane coupling agent KH560.
[0039] Based on about 100 parts by weight of the halogen-free flame retardant polyamide elastomer material, the halogen-free flame retardant polyamide elastomer material may include about 0.4 parts by weight to about 2 parts by weight of the coupling agent, for example, 0.5 parts by weight, 1 part by weight, 1.5 parts by weight, or 2 parts by weight.
[0040] Dispersants
[0041] The dispersant can be one or more of ethylene bis stearamide, stearic acid monoglyceride, tristearic acid glyceride, oleamide, mesoamide, polyethylene wax, liquid paraffin, metal salts of higher fatty acids, pentaerythritol stearate, etc., preferably pentaerythritol stearate (PETS). The addition of dispersant is also crucial. Dispersant, with its double electrical layer principle and steric hindrance effect, makes material form a stable and uniform dispersion system, thereby improving material performance.
[0042] Based on about 100 parts by weight of the halogen-free flame retardant polyamide elastomer material, the halogen-free flame retardant polyamide elastomer material may include about 0.5 parts by weight to about 3 parts by weight of the dispersant, for example, 0.5 parts by weight, 1 part by weight, 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, or 3 parts by weight.
[0043] Compatibilizer
[0044] The compatibilizer can be a mixture of one or more of a cyclic anhydride compatibilizer, an epoxy compatibilizer, and an oxazoline compatibilizer, preferably a cyclic anhydride compatibilizer, and can be a maleic anhydride grafted styrene-ethylene-butadiene-styrene block copolymer elastomer (SEBS-g-MAH) (wherein SEBS is divided into linear and star-shaped, preferably linear SEBS, with a molecular weight of ≥70,000), a maleic anhydride grafted ethylene-octene copolymer (POE-g-MAH), preferably SEBS-g-MAH, and the maleic anhydride (MAH) grafting rate is 0.5%-3%.
[0045] Based on about 100 parts by weight of the halogen-free flame retardant polyamide elastomer material, the halogen-free flame retardant polyamide elastomer material may include about 3 parts by weight to about 10 parts by weight of a compatibilizer, for example, 3 parts by weight, 4 parts by weight, 5 parts by weight, 6 parts by weight, 7 parts by weight, 8 parts by weight, 9 parts by weight, or 10 parts by weight.
[0046] The amount of compatibilizer added and the amount of grafting are within a certain range and cannot be too low or too high. If the amount of addition is too low or too high, the compatibility of the entire system is poor, which will lead to a decrease in the mechanical properties and flame retardancy of the composite material. If the amount of grafting is too high, it will cause a cross-linking reaction of the base resin and the composite material will lose plasticity. In addition, the present invention also finds that the addition of an elastomer compatibilizer can build a "bridge" between the flame retardant and the polyamide elastomer, which plays a role in reducing interfacial tension, increasing the thickness of the interface layer, and reducing the size of dispersed particles, so that the system finally forms a thermodynamically stable phase structure with macroscopically uniform microscopic phase separation characteristics, thereby improving the mechanical properties of the material.
[0047] Antioxidants
[0048] The antioxidant may be one or more of antioxidant 168, antioxidant 1010, antioxidant 1076, antioxidant 1098, antioxidant 3114, antioxidant 164, antioxidant 264, antioxidant BHT, antioxidant T501, antioxidant B215, and antioxidant B225.
[0049] Based on about 100 parts by weight of the halogen-free flame retardant polyamide elastomer material, the halogen-free flame retardant polyamide elastomer material may include about 0.1 parts by weight to about 1 parts by weight of an antioxidant, for example, 0.1 parts by weight, 0.2 parts by weight, 0.3 parts by weight, 0.4 parts by weight, 0.5 parts by weight, 0.6 parts by weight, 0.8 parts by weight, or 1 part by weight.
[0050] Absorbent
[0051] The absorbent may be one or more of nano titanium dioxide, porous silicate, diatomaceous earth, zinc ricinoleate, zinc sulfate, and nano zinc oxide, preferably porous silicate. The phosphorus-based flame retardant used in the present invention is halogen-free, environmentally friendly, and highly efficient, but a small amount of highly toxic gases such as PH3 will still be produced during the flame retardant decomposition process, which will have an impact on the human body and the environment. The porous silicate in this system can well capture the gases such as PH3 produced in the combustion chamber, and at the same time form a non-combustible mineral layer on the surface of the polymer, which has a synergistic flame retardant effect on the system.
[0052] Based on about 100 parts by weight of the halogen-free flame retardant polyamide elastomer material, the halogen-free flame retardant polyamide elastomer material may include about 0.1 parts by weight to about 2 parts by weight of the absorbent, for example, 0.1 parts by weight, 0.2 parts by weight, 0.4 parts by weight, 0.6 parts by weight, 0.8 parts by weight, 1 part by weight, 1.2 parts by weight, 1.5 parts by weight, 1.8 parts by weight, or 2 parts by weight.
[0053] Another aspect of the present invention provides a method for preparing the halogen-free flame-retardant polyamide elastomer material, comprising one of the following methods:
[0054] Method 1:
[0055] (1) mixing a main flame retardant, a synergistic flame retardant, a coupling agent and a compatibilizer to obtain material A;
[0056] (2) adding a polyamide elastomer, a dispersant, an antioxidant and an absorbent to material A and continuing to mix to obtain material B;
[0057] (3) Material B is melt-kneaded, extruded, and granulated to obtain a halogen-free flame-retardant polyamide elastomer material.
[0058] In some embodiments, the mixing temperature in step (1) is 75 to 85°C;
[0059] In some embodiments, step (2) includes: first adding polyamide elastomer to material A for first mixing, and then continuing to add dispersant, antioxidant and absorbent for second mixing, the temperature of the first mixing is 75-90° C., and the temperature of the second mixing is 95-110° C.;
[0060] In some embodiments, in step (2), the mixing time to reach the specified temperature is 3-10 min, preferably 5-8 min.
[0061] In some embodiments, the melt mixing temperature in step (3) is 210-240°C.
[0062] Method 2:
[0063] (1) firstly, a part (e.g., 50-65% by weight of the total weight of the polyamide elastomer) of the polyamide elastomer, the main flame retardant, the synergistic flame retardant, the coupling agent, the compatibilizer, the dispersant, the antioxidant and the absorbent are put into an internal mixer and mixed for a period of time to prepare a master batch, and the mixing temperature is controlled at 180-200° C.;
[0064] (2) After the master batch and the remaining part of the polyamide elastomer are uniformly mixed, they are extruded into granules by a twin-screw extruder; or, the master batch and the polyamide elastomer are further kneaded, and then extruded into granules by a single-screw extruder.
[0065] The polyamide elastomer mixture is processed by a low shear parallel twin-screw extruder, a mixing single-screw extruder, or a reciprocating extruder.
[0066] The extruder is a low shear extrusion screw.
[0067] The present invention provides a polyamide elastomer material and a preparation method thereof, which uses a polyamide elastomer as a substrate, is filled with aluminum hypophosphite, and is synergistically expanded and toughened with a zinc borate compatibilizer. The aluminum hypophosphite is combined with a synergistic flame retardant zinc borate, and after surface treatment with a coupling agent, the material has good compatibility with the polyamide elastomer material, and the system has synergistic flame retardancy, a small amount of addition, good hydrolysis stability, and is halogen-free, environmentally friendly, and smoke-suppressing, and has good mechanical properties and flame retardant and smoke-suppressing effects.
[0068] The halogen-free flame-retardant polyamide material prepared by this method has a flame retardancy not lower than V2 level, and even reaches V0 level. At the same time, the tensile strength is 30-45MPa, the elongation at break is more than 300%, and the impact strength is 45KJ / m 2 As described above, the flame retardant material of the present invention has excellent performance.
[0069] In another aspect, the present invention provides a use of the halogen-free flame-retardant polyamide elastomer material in preparing a halogen-free low-smoke flame-retardant cable or a flame-retardant injection molded part.
[0070] Beneficial effects:
[0071] 1) The present invention abandons traditional plastics and adopts polyamide elastomer as the base material of flame retardant material, which has excellent mechanical properties and low hardness, thus laying a foundation for the good mechanical properties, flexibility and low temperature resistance of the material system.
[0072] 2) The synergistic flame retardant system of aluminum hypophosphite and zinc borate of the present invention is halogen-free, smoke-suppressing, green and environmentally friendly, and has good hydrolysis stability.
[0073] 3) The present invention has good flame retardant effect and maintains the hardness of the original elastomer material.
[0074] The present invention has been described in detail above, but the above embodiments are only illustrative in nature and are not intended to limit the present invention. In addition, this article is not limited by any theory described in the above prior art or invention content or the following examples.
[0075] Unless otherwise expressly stated, the numerical ranges throughout the application documents include any subranges therein and any numerical values incremented by the smallest subunit of a given value therein. Unless otherwise expressly stated, the numerical values throughout the application documents represent approximate measurements or limitations of the range of embodiments including slight deviations from the given values and having approximately the values mentioned and having the exact values mentioned. Except for the working examples provided at the end of the detailed description, all numerical values of parameters (e.g., quantities or conditions) in this application document (including the appended claims) should be understood in all cases as modified by the term "approximately", regardless of whether "approximately" actually appears before the numerical value. "Approximately" means that the numerical value described allows for slight imprecision (some close to precision in the value; approximately or reasonably close to the value; approximately). If the imprecision provided by "approximately" is not understood in this ordinary sense in the art, the "approximately" used herein at least represents the variation that can be produced by ordinary methods of measuring and using these parameters. For example, "approximately" can include a variation of less than or equal to 10%, less than or equal to 5%, less than or equal to 4%, less than or equal to 3%, less than or equal to 2%, less than or equal to 1% or less than or equal to 0.5%. DETAILED DESCRIPTION
[0076] The present invention is further described below in conjunction with examples. It should be noted that the following examples are provided for illustrative purposes only and do not constitute a limitation on the scope of protection claimed for the present invention.
[0077] Unless otherwise specified, the raw materials, reagents, methods, etc. used in the examples are conventional raw materials, reagents, methods in the art.
[0078] raw material:
[0079] The homemade polyamide elastomer resin TPAE-6 (relative viscosity of about 2.0) is prepared by adding 20g of polyethylene glycol with a number average molecular weight of 2000, 80g of caprolactam, 3g of deionized water, 3g of sulfuric acid, and 1g of adipic acid into a reactor, heating to 240°C under nitrogen protection, and reacting at 800rpm for 1.5 hours; then, evacuating to 40Pa at 260°C and continuing to react at 800rpm for 2.5 hours, and then extracting with boiling water and drying.
[0080] Aluminum hypophosphite (AHP) was purchased from Suzhou Antefei New Materials Co., Ltd., AT-601 (whiteness 96, purity ≥98.5, particle size <5 μm);
[0081] Magnesium phosphate was purchased from Hubei Shineng Chemical Technology Co., Ltd., industrial grade;
[0082] Zinc borate (ZB) was purchased from Hefei Wanran New Material Technology Co., Ltd., environmentally friendly 8000 mesh;
[0083] Sb2O3 was purchased from Jiangsu Jimai Flame Retardant Material Technology Co., Ltd., Muli brand, high purity grade;
[0084] SEBS-g-MAH was purchased from Shell Kraton, FG1901GT (parameters: grafting rate about 1.7%);
[0085] Polyurethane (TPU) was purchased from Wanhua Chemical, WHT-8254;
[0086] Other TPAE6: Arkema PEBAX HD5513 SA01;
[0087] Coupling agent KH560 was purchased from Nanjing Feiteng New Materials Technology Co., Ltd.;
[0088] Dispersant / lubricant PETS was purchased from Dinghai Plastic Chemical Co., Ltd., Italy FACI brand PETS-AHS;
[0089] Antioxidants 1098 / 168 were purchased from BASF 1098 and 168 from Dinghai Plastic Chemical Co., Ltd.;
[0090] Porous silicate was purchased from Tianjin Yitailong Additive Company as magnesium silicate MS10E.
[0091] equipment:
[0092] High-speed mixer: HSM-50 Jiangsu Bell Machinery;
[0093] Parallel twin-screw extruder: HK36 Nanjing Keya Chemical Equipment Co., Ltd.;
[0094] Injection molding machine: UN120SM Guangdong Yizumi Precision Machinery Co., Ltd.
[0095] Electronic universal material testing machine: Zwick / Roell Z020 Shanghai Zwick Machinery Equipment Co., Ltd.;
[0096] Horizontal and vertical combustion tester: CZF-5 Beijing AVIC Times Instrument Equipment Co., Ltd.
[0097] Pendulum impact tester: Zwick / RoellHIT50P Shanghai Zwick Machinery Equipment Co., Ltd.;
[0098] Notching instrument: B1120.26.10 Shanghai Zwick Machinery Equipment Co., Ltd.
[0099] Example
[0100] Example 1
[0101] The method for preparing a halogen-free flame-retardant polyamide elastomer material comprises the following steps:
[0102] (1) 15 parts by weight of AHP, 15 parts by weight of ZB, 10 parts by weight of SEBS-g-MAH, and 0.5 parts by weight of silane coupling agent KH560 coupling agent (which can be diluted with 95% vol ethanol when added, the content represents the content before dilution, and the dilution volume ratio KH560:95% ethanol=1:5) are added into a high-speed mixer in a spray form and mixed at high speed while heating to 80° C. to obtain a flame retardant mixture with a surface treatment;
[0103] (2) 58.3 parts by weight of the homemade polyamide elastomer resin TPAE-6 is added to the surface-treated flame retardant mixture of step (1), and mixed at 85° C. in a high-speed mixer for 5 to 8 minutes. Then, 0.5 parts by weight of pentaerythritol stearate PETS, 0.4 parts by weight of an antioxidant mixture (0.2 parts by weight of antioxidant 1098 and 0.2 parts by weight of antioxidant 168), and 0.3 parts by weight of porous silicate are added, and the mixture is further fully blended at 100° C. for 5 to 8 minutes. The mixture is discharged to obtain a halogen-free flame-retardant polyamide elastomer raw material mixture.
[0104] (3) Add the above halogen-free flame-retardant polyamide elastomer raw material mixture into a parallel twin-screw extruder, perform melt-mixing and extrusion in a temperature range of 210 to 240° C., and obtain a halogen-free flame-retardant polyamide elastomer material after cooling and pelletizing.
[0105] Example 2
[0106] The method for preparing a halogen-free flame-retardant polyamide elastomer material comprises the following steps:
[0107] (1) 18 parts by weight of AHP, 12 parts by weight of ZB, 8 parts by weight of SEBS-g-MAH, and 0.5 parts by weight of silane coupling agent KH560 coupling agent (which can be diluted with 95% vol ethanol when added, the content represents the content before dilution, and the dilution volume ratio KH560:95% ethanol=1:5) are added into a high-speed mixer in a spray form and mixed at high speed while heating. After mixing to 80° C., a flame retardant mixture with a surface treatment is obtained;
[0108] (2) 59.5 parts by weight of the homemade polyamide elastomer resin TPAE-6 is added to the flame retardant mixture that has been surface treated in step (1), and mixed at 85° C. in a high-speed mixer for 5 to 8 minutes. Then, 1 part by weight of pentaerythritol stearate PETS, 0.5 part by weight of an antioxidant mixture (0.2 part by weight of antioxidant 1098 and 0.3 part by weight of antioxidant 168), and 0.5 part by weight of porous silicate are added, and the mixture is further fully blended at 100° C. for 5 to 8 minutes. The mixture is discharged to obtain a halogen-free flame-retardant polyamide elastomer raw material mixture.
[0109] (3) Add the above halogen-free flame-retardant polyamide elastomer raw material mixture into a parallel twin-screw extruder, perform melt-mixing and extrusion in a temperature range of 210 to 240° C., and obtain a halogen-free flame-retardant polyamide elastomer material after cooling and pelletizing.
[0110] Example 3
[0111] The method for preparing a halogen-free flame-retardant polyamide elastomer material comprises the following steps:
[0112] (1) 20 parts by weight of AHP, 10 parts by weight of ZB, 5 parts by weight of SEBS-g-MAH, and 0.6 parts by weight of silane coupling agent KH560 coupling agent (which can be diluted with 95% vol ethanol when added, the content represents the content before dilution, and the dilution volume ratio KH560:95% ethanol=1:5) are added into a high-speed mixer in a spray form and mixed at high speed while heating. After mixing to 80° C., a flame retardant mixture with a surface treatment is obtained;
[0113] (2) 61.8 parts by weight of the homemade polyamide elastomer resin TPAE-6 is added to the flame retardant mixture that has been surface treated in step (1), and mixed at 85° C. in a high-speed mixer for 5 to 8 minutes. Then, 2 parts by weight of pentaerythritol stearate PETS, 0.3 parts by weight of an antioxidant mixture (0.1 parts by weight of antioxidant 1098 and 0.2 parts by weight of antioxidant 168), and 0.3 parts by weight of porous silicate are added, and the mixture is further fully blended at 100° C. for 5 to 8 minutes. The mixture is discharged to obtain a halogen-free flame-retardant polyamide elastomer raw material mixture.
[0114] (3) Add the above halogen-free flame-retardant polyamide elastomer raw material mixture into a parallel twin-screw extruder, perform melt-mixing and extrusion in a temperature range of 210 to 240° C., and obtain a halogen-free flame-retardant polyamide elastomer material after cooling and pelletizing.
[0115] Example 4
[0116] The method for preparing a halogen-free flame-retardant polyamide elastomer material comprises the following steps:
[0117] (1) 22 parts by weight of AHP, 8 parts by weight of ZB, 5 parts by weight of SEBS-g-MAH, and 0.6 parts by weight of silane coupling agent KH560 coupling agent (which can be diluted with 95% vol ethanol when added, the content represents the content before dilution, and the dilution volume ratio KH560:95% ethanol=1:5) are added into a high-speed mixer in a spray form and mixed at high speed while heating. After mixing to 80° C., a flame retardant mixture with a surface treatment is obtained;
[0118] (2) 62.5 parts by weight of the homemade polyamide elastomer resin TPAE-6 is added to the flame retardant mixture that has been surface treated in step (1), and mixed at 85° C. in a high-speed mixer for 5 to 8 minutes. Then, 1 part by weight of pentaerythritol stearate PETS, 0.5 part by weight of an antioxidant mixture (0.2 part by weight of antioxidant 1098 and 0.3 part by weight of antioxidant 168), and 0.4 part by weight of porous silicate are added, and the mixture is further fully blended at 100° C. for 5 to 8 minutes. The mixture is discharged to obtain a halogen-free flame-retardant polyamide elastomer raw material mixture.
[0119] (3) Add the above halogen-free flame-retardant polyamide elastomer raw material mixture into a parallel twin-screw extruder, perform melt-mixing and extrusion in a temperature range of 210 to 240° C., and obtain a halogen-free flame-retardant polyamide elastomer material after cooling and pelletizing.
[0120] Example 5
[0121] The method for preparing a halogen-free flame-retardant polyamide elastomer material comprises the following steps:
[0122] (1) 25 parts by weight of AHP, 6 parts by weight of ZB, 3 parts by weight of SEBS-g-MAH, and 0.6 parts by weight of silane coupling agent KH560 coupling agent (which can be diluted with 95% vol ethanol when added, the content represents the content before dilution, and the dilution volume ratio KH560:95% ethanol=1:5) are added into a high-speed mixer in a spray form and mixed at high speed while heating. After mixing to 80° C., a flame retardant mixture with a surface treatment is obtained;
[0123] (2) 62.8 parts by weight of the homemade polyamide elastomer resin TPAE-6 is added to the flame retardant mixture that has been surface treated in step (1), and mixed at 85° C. in a high-speed mixer for 5 to 8 minutes. Then, 1 part by weight of pentaerythritol stearate PETS, 0.6 part by weight of an antioxidant mixture (0.2 part by weight of antioxidant 1098 and 0.4 part by weight of antioxidant 168), and 1 part by weight of porous silicate are added, and the mixture is further fully blended at 100° C. for 5 to 8 minutes. The mixture is discharged to obtain a halogen-free flame-retardant polyamide elastomer raw material mixture.
[0124] (3) Add the above halogen-free flame-retardant polyamide elastomer raw material mixture into a parallel twin-screw extruder, perform melt-mixing and extrusion in a temperature range of 210 to 240° C., and obtain a halogen-free flame-retardant polyamide elastomer material after cooling and pelletizing.
[0125] Example 6
[0126] The method for preparing a halogen-free flame-retardant polyamide elastomer material comprises the following steps:
[0127] (1) 25 parts by weight of AHP, 3 parts by weight of ZB, 6 parts by weight of SEBS-g-MAH, and 0.4 parts by weight of silane coupling agent KH560 coupling agent (which can be diluted with 95% vol ethanol when added, the content represents the content before dilution, and the dilution volume ratio KH560:95% ethanol=1:5) are added into a high-speed mixer in a spray form and mixed at high speed while heating. After mixing to 80° C., a flame retardant mixture with a surface treatment is obtained;
[0128] (2) 62.6 parts by weight of the homemade polyamide elastomer resin TPAE-6 is added to the flame retardant mixture that has been surface treated in step (1), and mixed at 85° C. in a high-speed mixer for 5 to 8 minutes. Then, 1 part by weight of pentaerythritol stearate PETS, 0.5 parts by weight of an antioxidant mixture (0.2 parts by weight of antioxidant 1098 and 0.3 parts by weight of antioxidant 168), and 1.5 parts by weight of porous silicate are added, and the mixture is further fully blended at 100° C. for 5 to 8 minutes. The mixture is discharged to obtain a halogen-free flame-retardant polyamide elastomer raw material mixture.
[0129] (3) Add the above halogen-free flame-retardant polyamide elastomer raw material mixture into a parallel twin-screw extruder, perform melt-mixing and extrusion in a temperature range of 210 to 240° C., and obtain a halogen-free flame-retardant polyamide elastomer material after cooling and pelletizing.
[0130] Comparative Example 1
[0131] The method for preparing a halogen-free flame-retardant polyamide elastomer material comprises the following steps:
[0132] (1) 22 parts by weight of AHP, 8 parts by weight of ZB, 5 parts by weight of SEBS-g-MAH, and 0.6 parts by weight of silane coupling agent KH560 coupling agent (which can be diluted with 95% vol ethanol when added, the content represents the content before dilution, and the dilution volume ratio KH560:95% ethanol=1:5) are added into a high-speed mixer in a spray form and mixed at high speed while heating to 80° C. to obtain a flame retardant mixture with a surface treatment;
[0133] (2) Add 62.5 parts by weight of PEBAX 5513SA01 to the flame retardant mixture surface-treated in step (1), mix at 85° C. in a high-speed mixer for 5 to 8 minutes, then add 1 part by weight of pentaerythritol stearate PETS, 0.5 part by weight of an antioxidant mixture (0.2 part by weight of antioxidant 1098 and 0.3 part by weight of antioxidant 168), and 0.4 part by weight of porous silicate, continue to fully blend at 100° C. for 5 to 8 minutes, and discharge to obtain a halogen-free flame retardant polyamide elastomer raw material mixture.
[0134] (3) Add the above halogen-free flame-retardant polyamide elastomer raw material mixture into a parallel twin-screw extruder, perform melt-mixing and extrusion in a temperature range of 210 to 240° C., and obtain a halogen-free flame-retardant polyamide elastomer material after cooling and pelletizing.
[0135] Comparative Example 2
[0136] The method for preparing a halogen-free flame-retardant polyurethane elastomer material comprises the following steps:
[0137] (1) 22 parts by weight of AHP, 8 parts by weight of ZB, 5 parts by weight of SEBS-g-MAH, and 0.6 parts by weight of silane coupling agent KH560 coupling agent (which can be diluted with 95% vol ethanol when added, the content represents the content before dilution, and the dilution volume ratio KH560:95% ethanol=1:5) are added into a high-speed mixer in a spray form and mixed at high speed while heating. After mixing to 80° C., a flame retardant mixture with a surface treatment is obtained;
[0138] (2) Add 62.5 parts by weight of polyurethane elastomer resin TPU to the surface-treated flame retardant mixture of step (1), mix at 85° C. in a high-speed mixer for 5 to 8 minutes, then add 1 part by weight of pentaerythritol stearate PETS, 0.5 part by weight of an antioxidant mixture (0.2 part by weight of antioxidant 1098 and 0.3 part by weight of antioxidant 168), and 0.4 part by weight of porous silicate, continue to fully blend at 100° C. for 5 to 8 minutes, and discharge the mixture to obtain a halogen-free flame retardant polyurethane elastomer raw material mixture.
[0139] (3) Add the above halogen-free flame-retardant polyurethane elastomer raw material mixture into a parallel twin-screw extruder, perform melt-mixing and extrusion in a temperature range of 180 to 210° C., and obtain a halogen-free flame-retardant polyurethane elastomer material after cooling and pelletizing.
[0140] Comparative Example 3
[0141] The method for preparing a halogen-free flame-retardant polyamide elastomer material comprises the following steps:
[0142] (1) 30 parts by weight of AHP, 5 parts by weight of SEBS-g-MAH, and 0.6 parts by weight of silane coupling agent KH560 coupling agent (which can be diluted with 95% vol ethanol when added, the content represents the content before dilution, and the dilution volume ratio KH560:95% ethanol=1:5) are added into a high-speed mixer in a spray form and mixed at high speed while heating. After mixing to 80° C., a flame retardant mixture with a surface treatment is obtained;
[0143] (2) 62.5 parts by weight of the homemade polyamide elastomer resin TPAE-6 is added to the flame retardant mixture that has been surface treated in step (1), and mixed at 85° C. in a high-speed mixer for 5 to 8 minutes. Then, 1 part by weight of pentaerythritol stearate PETS, 0.5 part by weight of an antioxidant mixture (0.2 part by weight of antioxidant 1098 and 0.3 part by weight of antioxidant 168), and 0.4 part by weight of porous silicate are added, and the mixture is further fully blended at 100° C. for 5 to 8 minutes. The mixture is discharged to obtain a halogen-free flame-retardant polyamide elastomer raw material mixture.
[0144] (3) Add the above halogen-free flame-retardant polyamide elastomer raw material mixture into a parallel twin-screw extruder, perform melt-mixing and extrusion in a temperature range of 210 to 240° C., and obtain a halogen-free flame-retardant polyamide elastomer material after cooling and pelletizing.
[0145] Comparative Example 4
[0146] The method for preparing a halogen-free flame-retardant polyurethane elastomer material comprises the following steps:
[0147] (1) 22 parts by weight of AHP, 8 parts by weight of Sb2O3, 5 parts by weight of SEBS-g-MAH, and 0.6 parts by weight of silane coupling agent KH560 coupling agent (which can be diluted with 95% vol ethanol when added, the content represents the content before dilution, and the dilution volume ratio KH560:95% ethanol=1:5) are added into a high-speed mixer in a spray form and mixed at high speed while heating. After mixing to 80° C., a flame retardant mixture with a surface treatment is obtained;
[0148] (2) 62.5 parts by weight of the homemade polyamide elastomer resin TPAE-6 is added to the surface-treated flame retardant mixture of step (1), and mixed at 85° C. in a high-speed mixer for 5 to 8 minutes. Then, 1 part by weight of pentaerythritol stearate PETS, 0.5 part by weight of an antioxidant mixture (0.2 part by weight of antioxidant 1098 and 0.3 part by weight of antioxidant 168), and 0.4 part by weight of porous silicate are added, and the mixture is further fully blended at 100° C. for 5 to 8 minutes. The mixture is discharged to obtain a halogen-free flame retardant polyurethane elastomer raw material mixture.
[0149] (3) Add the above halogen-free flame-retardant polyurethane elastomer raw material mixture into a parallel twin-screw extruder, perform melt-mixing and extrusion in a temperature range of 180 to 210° C., and obtain a halogen-free flame-retardant polyurethane elastomer material after cooling and pelletizing.
[0150] Comparative Example 5
[0151] The method for preparing a halogen-free flame-retardant polyurethane elastomer material comprises the following steps:
[0152] (1) 22 parts by weight of AHP, 8 parts by weight of ZB, 5 parts by weight of SEBS-g-MAH, and 0.6 parts by weight of silane coupling agent KH560 coupling agent (which can be diluted with 95% vol ethanol when added, the content represents the content before dilution, and the dilution volume ratio KH560:95% ethanol=1:5) are added into a high-speed mixer in a spray form and mixed at high speed while heating. After mixing to 80° C., a flame retardant mixture with a surface treatment is obtained;
[0153] (2) 62.9 parts by weight of the homemade polyamide elastomer resin TPAE-6 is added to the flame retardant mixture that has been surface treated in step (1), and mixed at 85° C. in a high-speed mixer for 5 to 8 minutes. Then, 1 part by weight of pentaerythritol stearate PETS and 0.5 part by weight of an antioxidant mixture (0.2 parts by weight of antioxidant 1098 and 0.3 parts by weight of antioxidant 168) are added, and the mixture is further fully blended at 100° C. for 5 to 8 minutes. The mixture is discharged to obtain a halogen-free flame retardant polyurethane elastomer raw material mixture.
[0154] (3) Add the above halogen-free flame-retardant polyurethane elastomer raw material mixture into a parallel twin-screw extruder, perform melt-mixing and extrusion in a temperature range of 180 to 210° C., and obtain a halogen-free flame-retardant polyurethane elastomer material after cooling and pelletizing.
[0155] Comparative Example 6
[0156] The method for preparing a halogen-free flame-retardant polyamide elastomer material comprises the following steps:
[0157] (1) 22 parts by weight of magnesium phosphate, 8 parts by weight of ZB, 5 parts by weight of SEBS-g-MAH, and 0.6 parts by weight of silane coupling agent KH560 coupling agent (which can be diluted with 95% vol ethanol when added, the content represents the content before dilution, and the dilution volume ratio KH560:95% ethanol=1:5) are added in a high-speed mixer in a spray form and mixed at high speed while heating to 80° C. to obtain a flame retardant mixture with a surface treatment;
[0158] (2) 62.5 parts by weight of the homemade polyamide elastomer resin TPAE-6 is added to the flame retardant mixture that has been surface treated in step (1), and mixed at 85° C. in a high-speed mixer for 5 to 8 minutes. Then, 1 part by weight of pentaerythritol stearate PETS, 0.5 part by weight of an antioxidant mixture (0.2 part by weight of antioxidant 1098 and 0.3 part by weight of antioxidant 168), and 0.4 part by weight of porous silicate are added, and the mixture is further fully blended at 100° C. for 5 to 8 minutes. The mixture is discharged to obtain a halogen-free flame-retardant polyamide elastomer raw material mixture.
[0159] (3) Add the above halogen-free flame-retardant polyamide elastomer raw material mixture into a parallel twin-screw extruder, perform melt-mixing and extrusion in a temperature range of 210 to 240° C., and obtain a halogen-free flame-retardant polyamide elastomer material after cooling and pelletizing.
[0160] Comparative Example 7
[0161] The method for preparing a halogen-free flame-retardant polyurethane elastomer material comprises the following steps:
[0162] (1) 22 parts by weight of AHP, 8 parts by weight of ZB, and 0.6 parts by weight of silane coupling agent KH560 coupling agent (which can be diluted with 95% vol ethanol when added, the content represents the content before dilution, and the dilution volume ratio KH560:95% ethanol=1:5) are added into a high-speed mixer in a spray form and mixed at high speed while heating to 80° C. to obtain a flame retardant mixture with a surface treatment;
[0163] (2) 67.5 parts by weight of the homemade polyamide elastomer resin TPAE-6 is added to the surface-treated flame retardant mixture of step (1), and mixed at 85° C. for 5 to 8 minutes in a high-speed mixer. Then, 1 part by weight of pentaerythritol stearate PETS, 0.5 part by weight of an antioxidant mixture (0.2 part by weight of antioxidant 1098 and 0.3 part by weight of antioxidant 168), and 0.4 part by weight of porous silicate are added, and the mixture is further fully blended at 100° C. for 5 to 8 minutes. The mixture is discharged to obtain a halogen-free flame retardant polyurethane elastomer raw material mixture.
[0164] (3) Add the above halogen-free flame-retardant polyurethane elastomer raw material mixture into a parallel twin-screw extruder, perform melt-mixing and extrusion in a temperature range of 180 to 210° C., and obtain a halogen-free flame-retardant polyurethane elastomer material after cooling and pelletizing.
[0165] The specific formulations of the embodiments and comparative examples are shown in Table 1:
[0166] Table 1
[0167]
[0168]
[0169] Unit: weight parts
[0170] Experimental example: Mechanical properties and flame retardant properties test
[0171] The flame retardant properties and mechanical properties of the composite materials of Examples 1-6 and Comparative Examples 1-7 were tested. The test results are shown in Table 2. The performance evaluation method and test standard are as follows:
[0172] The extruded granulated composite material was dried at 90° C. for 1 to 2 hours, and then the test samples were molded using an injection molding machine equipped with a standard test specimen mold (each group of samples contained 5 tensile and impact test specimens and 5 flame retardant test specimens).
[0173] Mechanical properties test: According to the ASTM D638-2003 plastic tensile properties test standard of the American Society for Testing and Materials, the tensile properties of the samples were tested using an electronic universal tensile testing machine. At least 5 parallel samples were required for each group of tensile tests, and the average value was taken.
[0174] The samples were tested according to the plastic cantilever beam impact standard in ISO180-2001. At least 5 parallel samples were required for each group of impact tests, and the average value of the results was taken (pendulum impact tester, notch tester).
[0175] Flame retardant performance test: The open flame flame retardant performance was tested according to the UL94-2006 standard, and the sample standard was 125×15×1.6mm (horizontal vertical combustion tester).
[0176] Table 2
[0177]
[0178] Conclusion: The flame retardant and mechanical test results show that the raw materials, additives and proportions used in Examples 4 and 3 are the most ideal, which can meet the ideal flame retardant requirements of the materials and have excellent mechanical properties. It can be seen from the above table that aluminum hypophosphite and zinc borate, when added at a ratio of about 2 to 3:1 and the total mass fraction reaches about 25 to 35, achieve the most ideal flame retardant effect, and are low-smoke, halogen-free and environmentally friendly, and are an ideal halogen-free flame retardant elastomer material. In the proportions within the scope of the embodiment, the materials all show good flame retardant and mechanical properties. In Comparative Example 1, the substrate is replaced with PEBAX HD 5513, which has slightly worse compatibility with flame retardants than TPAE6 and slightly worse performance. In Comparative Example 2, a halogen-free flame retardant material is prepared using a commonly used polyurethane elastomer on the market. With the same addition and proportion, its flame retardant performance is comparable to that of a polyamide elastomer resin, but its tensile strength is quite different from that of a flame retardant composite material with a polyamide elastomer substrate, showing the good mechanical properties of polyamide elastomers. In Comparative Example 3, the synergistic flame retardant zinc borate was not added, and the flame retardant performance of the material was not enough compared with the same period last year. In Comparative Example 4, the synergistic flame retardant was replaced with antimony trioxide. In this flame retardant system, the synergistic function of antimony trioxide was not obvious, and the flame retardant performance of the material was relatively poor. In Comparative Example 5, no absorbent was added, resulting in the acidic gas produced by this flame retardant system not being absorbed. Although there was a certain gas phase flame retardant effect, these gases had a catalytic effect on the combustion decomposition reaction, resulting in slightly poor flame retardant performance of the material and the release of a certain odor. In Comparative Example 6, the main flame retardant aluminum hypophosphite was replaced with magnesium phosphate. The mechanical properties were not much different, but the flame retardant effect of the system was not ideal. In Comparative Example 7, the system had no compatibilizer, which also resulted in insufficient compatibility between the flame retardant and the substrate, and no toughening effect, and poor mechanical properties.
[0179] It can be seen that by selecting the resin substrate of the present invention, synergizing the flame retardant of zinc borate with aluminum hypophosphite, and selecting the appropriate amount of added compatibilizer SEBS-g-MAH and dispersant and absorbent, the material of the present invention exhibits an excellent balance between flame retardant properties and mechanical properties.
[0180] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A halogen-free flame-retardant polyamide elastomer material, characterized in that: The halogen-free flame-retardant polyamide elastomer material is mainly composed of the following components based on 100 parts by total weight: 55-75 parts of polyamide elastomer, 15-25 parts of main flame retardant, 3-15 parts of synergistic flame retardant, 0.4-2 parts of coupling agent, 0.5-3 parts of dispersant, 3-10 parts of compatibilizer, 0.1-1 parts of antioxidant, and 0.1-2 parts of absorbent; Wherein, the main flame retardant is aluminum hypophosphite; The synergistic flame retardant is zinc borate, The polyamide elastomer is a nylon 6 type polyether block polyamide, and the nylon 6 type polyether block polyamide is prepared by a method comprising the following steps: adding polyether / polyester, caprolactam, deionized water, a catalyst, and a diacid into a reactor, heating to 200-240° C. under nitrogen protection, and reacting for 0.5-2 hours under mechanical stirring; then vacuuming to 20-500 Pa at 250-280° C. and continuing mechanical stirring to react for 0.5-3 hours; then extracting with boiling water and drying to obtain a polyamide 6 thermoplastic elastomer resin, wherein the diacid is oxalic acid, malonic acid, succinic acid or adipic acid, and wherein the catalyst is phosphoric acid, sulfuric acid, or aminocaproic acid; and In the halogen-free flame-retardant polyamide elastomer material, the weight ratio of aluminum hypophosphite to zinc borate is 2-3:1, and the total weight of aluminum hypophosphite and zinc borate accounts for 25%-35% of the total weight of the halogen-free flame-retardant polyamide elastomer material.
2. The halogen-free flame-retardant polyamide elastomer material according to claim 1, characterized in that: The halogen-free flame-retardant polyamide elastomer material is mainly composed of the following components based on 100 parts by total weight: 60-65 parts of polyamide elastomer, 20-25 parts of main flame retardant, 8-10 parts of synergistic flame retardant, 0.4-0.6 parts of coupling agent, 1-2 parts of dispersant, 3-10 parts of compatibilizer, 0.3-0.6 parts of antioxidant and 0.3-0.5 parts of absorbent.
3. The halogen-free flame-retardant polyamide elastomer material according to claim 1, characterized in that: The halogen-free flame-retardant polyamide elastomer material mainly consists of the following components based on 100 parts by total weight: 62-65 parts of polyamide elastomer, 22-23 parts of main flame retardant, 8-9 parts of synergistic flame retardant, 0.5-0.6 parts of coupling agent, 1-2 parts of dispersant, 5-6 parts of compatibilizer, 0.3-0.5 parts of antioxidant and 0.3-0.4 parts of absorbent.
4. The halogen-free flame-retardant polyamide elastomer material according to any one of claims 1 to 3, characterized in that: The relative viscosity of the polyamide elastomer is 1.5-3.
0.
5. The halogen-free flame-retardant polyamide elastomer material according to any one of claims 1 to 3, characterized in that: The relative viscosity of the polyamide elastomer is 2.0-2.
8.
6. The halogen-free flame-retardant polyamide elastomer material according to claim 1, characterized in that: The polyether / polyester is one or more selected from polytetrahydrofuran, polyethylene glycol, polypropylene glycol or polyethylene glycol; and / or The number average molecular weight of the polyether / polyester is 300-8000; and / or Based on the total weight of polyether / polyester and caprolactam, the amount of the polyester / polyether is 10wt% to 60wt%; and / or Based on the total weight of polyether / polyester and caprolactam, the amount of caprolactam is 40wt% to 90wt%; and / or the amount of diacid is 1 to 10wt%; and / or the amount of catalyst is 0.1 to 4wt%; and / or the amount of deionized water is 0.5 to 4wt%; and / or The mechanical stirring speed is 100-800 rpm.
7. The halogen-free flame-retardant polyamide elastomer material according to claim 1, characterized in that: The particle size D90 of the aluminum hypophosphite is 2-5 μm; and / or The temperature at which the aluminum hypophosphite loses 1 wt% of its weight is greater than 300° C.; and / or The zinc borate is 3.5 hydrate zinc borate with a particle size of 1-3 μm.
8. The halogen-free flame-retardant polyamide elastomer material according to claim 1, characterized in that: The coupling agent is a silane coupling agent or a titanate coupling agent; and / or The compatibilizer is one or more selected from cyclic anhydride compatibilizers, epoxy compatibilizers, and oxazoline compatibilizers; and / or The dispersant is one or more selected from ethylene bis stearamide, stearic acid monoglyceride, tristearic acid glyceride, oleic acid amide, mesic acid amide, polyethylene wax, liquid paraffin, metal salts of higher fatty acids, and pentaerythritol stearate; and / or The antioxidant is one or more selected from the group consisting of antioxidant 168, antioxidant 1010, antioxidant 1076, antioxidant 1098, antioxidant 3114, antioxidant 164, antioxidant 264, antioxidant BHT, antioxidant T501, antioxidant B215, and antioxidant B225; and / or The absorbent is one or more selected from nano titanium dioxide, porous silicate, diatomaceous earth, zinc ricinoleate, zinc sulfate, and nano zinc oxide.
9. The halogen-free flame-retardant polyamide elastomer material according to claim 1, characterized in that: The coupling agent is silane coupling agent KH560; and / or The compatibilizer is one or more selected from maleic anhydride grafted styrene-ethylene-butadiene-styrene block copolymer elastomer, maleic anhydride grafted ethylene-octene copolymer, maleic anhydride grafted ethylene-vinyl acetate copolymer, wherein the grafting rate of maleic anhydride is 0.5%-3%; and / or The absorbent is porous silicate.
10. The method for preparing the halogen-free flame-retardant polyamide elastomer material according to any one of claims 1 to 9, characterized in that: One of the following methods: Method 1: (1) mixing a main flame retardant, a synergistic flame retardant, a coupling agent and a compatibilizer to obtain material A; (2) adding a polyamide elastomer, a dispersant, an antioxidant and an absorbent to material A and continuing to mix to obtain material B; (3) melt-mixing, extruding and granulating the material B to obtain a halogen-free flame-retardant polyamide elastomer material; Method 2: (1') firstly, a part of the polyamide elastomer, the main flame retardant, the synergistic flame retardant, the compatibilizer, the dispersant, the antioxidant and the absorbent are put into an internal mixer and kneaded for a period of time to prepare a master batch; (2') After the master batch and the remaining part of the polyamide elastomer are uniformly mixed, the mixture is extruded into granules by a twin-screw extruder; or, the master batch and the polyamide elastomer are further kneaded, and then extruded into granules by a single-screw extruder.
11. The preparation method according to claim 10, characterized in that: The mixing temperature in step (1) is 75 to 85° C.; and / or Step (2) comprises: firstly adding polyamide elastomer to material A for first mixing, and then continuously adding dispersant, antioxidant and absorbent for second mixing, wherein the temperature of the first mixing is 75-90° C., and the temperature of the second mixing is 95-110° C.; and / or The melt mixing temperature in step (3) is 210 to 240° C.; and / or The banburying temperature in step (1') is 180-200°C.
12. Use of the halogen-free flame-retardant polyamide elastomer material according to any one of claims 1 to 9 in preparing halogen-free low-smoke flame-retardant cables or flame-retardant injection molded parts.