Method for recovering rare earth and niobium from fluorite concentrate

By performing pre-reaction and high-temperature treatment in fluorite concentrate, combined with water leaching and neutralization treatment, the recovery rate of rare earths and niobiums was successfully improved, the problem of underutilization of resources in the existing technology was solved, and efficient Rare earth and niobium recovery and high purity gypsum production.

CN115852174BActive Publication Date: 2024-11-05BAOTOU RESEARCH INSTITUTE OF RARE EARTHS +1
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202211522619.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-30
Publication Date
2024-11-05
Estimated Expiration
2042-11-30

AI Technical Summary

Technical Problem

The prior art failed to effectively recover rare earths and niobium in fluorite concentrate, resulting in underutilization of resources.

Method used

The dried fluorite concentrate particles are mixed with sulfuric acid for pre-reaction, and then reacted at high temperature to obtain the reaction gas and reaction slag, and leaching is made through water to obtain a leachate containing rare earths and niobium, and neutralize and magnetize with magnesium oxide. Machine selection treatment to improve the leaching rate of rare earths and niobium.

Benefits of technology

High-efficiency recovery of rare earths and niobiums was achieved, with the leaching rate of rare earths reaching 99.3%, and the leaching rate of niobium can reach 88.6%, and high-purity gypsum and anhydrous hydrogen fluoride were obtained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003971802700000101
    Figure BDA0003971802700000101
Patent Text Reader

Abstract

The invention discloses a method for recovering rare earth and niobium from fluorite concentrate, comprising the following steps: 1) mixing dried fluorite concentrate particles with sulfuric acid and pre-reacting at 90-150°C to obtain pre-reaction material; 2) reacting the pre-reaction material at 190-280°C to obtain reaction gas and reaction slag; 3) leaching the reaction slag with water to obtain a leaching solution containing rare earth and niobium and leaching slag; wherein the CaF2 content in the fluorite concentrate particles is greater than 75wt%, the REO content is 5.02-9wt%, and the Nb2O5 content is 0.05-0.5wt%; wherein the mass ratio of water to reaction slag is 0.14-0.25:1. The method has a high leaching rate of rare earth and niobium.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for recovering rare earth and niobium from fluorite concentrate. Background Art

[0002] Fluorite is an important non-metallic strategic mineral resource. The reserves of associated fluorite in the Bayan Obo mine rank first in China. However, due to the fine fluorite particles, complex embedding characteristics, high inclusion content, and many similar floatable minerals, the quality of fluorite concentrate is low, and it contains valuable resources such as rare earths and niobium, which are not fully utilized. Comprehensive resource utilization of this type of fluorite concentrate and further recovery of valuable metals in it have important economic value and environmental benefits.

[0003] CN109371239A discloses a method for treating low-grade fluorite ore containing rare earths. The method adopts a method of absolute excess sulfuric acid solution programmed temperature controlled segmented slurry decomposition treatment, controls the low temperature section to preferentially decompose fluorite minerals, raises the temperature to decompose rare earth minerals, recovers hydrofluoric acid from tail gas, and uses water to leach rare earths from the acid leaching residue after the reaction, neutralizes and removes thorium, and then recovers rare earths and gypsum. The rare earth content in the patent document is 1-5wt%, and only the REO decomposition rate is mentioned, without involving the leaching rate of rare earths and niobium.

[0004] CN113735062A discloses a method for preparing hydrogen fluoride by recycling fluorite from rare earths. The method first processes fluorite into powder and refines it into high-purity acid-grade fluorite concentrate, which is then reacted with industrial sulfuric acid to prepare high-purity hydrogen fluoride. The raw material is high-purity acid-grade fluorite concentrate. Although the ratio of fuming acid is mentioned in the production process, the specific value and the specific reaction temperature are not mentioned. More importantly, the recovery of rare earths and niobium is not considered.

[0005] CN102925670A discloses a method for comprehensively recovering fluorine and tungsten from tungsten-containing fluorite minerals. The method uses sulfuric acid and phosphoric acid to roast the tungsten-containing fluorite minerals to obtain hydrofluoric acid and recover tungsten respectively, but does not involve the recovery of rare earths and niobium. Summary of the invention

[0006] In view of this, an object of the present invention is to provide a method for recovering rare earth and niobium from fluorite concentrate, wherein the leaching rate of rare earth and niobium is high.

[0007] The present invention adopts the following technical solutions to achieve the above-mentioned purpose.

[0008] The present invention provides a method for recovering rare earth and niobium from fluorite concentrate, comprising the following steps:

[0009] 1) Mixing the dried fluorite concentrate particles with sulfuric acid and pre-reacting at 90-150° C. to obtain a pre-reaction material;

[0010] 2) reacting the pre-reaction material at 190-280° C. to obtain reaction gas and reaction slag;

[0011] 3) leaching the reaction slag with water to obtain a leaching solution containing rare earth and niobium and a leaching slag;

[0012] The CaF2 content in the fluorite concentrate particles is greater than 75wt%, the REO content is 5.02-9wt%, and the Nb2O5 content is 0.05-0.5wt%;

[0013] Among them, the mass ratio of water to reaction slag is 0.14-0.25:1.

[0014] According to the method of the present invention, preferably, in step 1), the sulfuric acid is a mixture of 98 wt % concentrated sulfuric acid and 105 wt % oleum;

[0015] The mass ratio of the dried fluorite concentrate particles, 98wt% concentrated sulfuric acid and 105wt% oleum is 1:(0.7-0.9):(0.6-0.8).

[0016] According to the method of the present invention, preferably, in step 1), the pre-reaction temperature is 100-140° C. and the pre-reaction time is 4-10 min.

[0017] According to the method of the present invention, preferably, in step 2), the pre-reaction material is reacted at 190-280° C. for 55-110 min to obtain a reaction gas containing hydrogen fluoride and a reaction slag.

[0018] According to the method of the present invention, preferably, in step 2), the reaction temperature is 220-260° C.; and the reaction time is 60-100 min.

[0019] The method according to the present invention preferably further comprises the following steps: washing the reaction gas containing hydrogen fluoride through a washing tower, and then condensing and rectifying to obtain anhydrous hydrogen fluoride.

[0020] According to the method of the present invention, preferably, in step 3), the mass ratio of water to reaction slag is 0.15-0.22:1.

[0021] The method according to the present invention preferably further comprises the following steps:

[0022] The leaching solution containing rare earth and niobium obtained in step 3) is neutralized with magnesium oxide to obtain a neutralized leaching solution containing rare earth and niobium and a neutralized slag;

[0023] The leached residue obtained in step 3) is subjected to magnetic separation by a magnetic separator to obtain calcium sulfate; wherein the magnetic separation intensity is 3.5 to 4.5 T; and the purity of the obtained calcium sulfate is greater than or equal to 90 wt%.

[0024] According to the method of the present invention, preferably, the dried fluorite concentrate particles are obtained by pretreatment comprising the following steps:

[0025] The fluorite concentrate is made into balls with a diameter of 2 to 5 mm, and the prepared balls are dried at 90 to 120° C. for 12 to 36 hours to obtain dried fluorite concentrate particles.

[0026] According to the method of the present invention, preferably, the leaching rate of rare earth is greater than or equal to 98.5%, and the leaching rate of niobium is greater than or equal to 85%.

[0027] The method of the present invention can recover rare earth and niobium from fluorite concentrate, and the leaching rates of rare earth and niobium are relatively high. The leaching rate of rare earth can reach 99.3%, and the leaching rate of niobium can reach 88.6%. In addition, the present invention can also obtain gypsum with a purity of more than 90% and obtain anhydrous hydrogen fluoride. DETAILED DESCRIPTION

[0028] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.

[0029] The method for recovering rare earth and niobium from fluorite concentrate of the present invention comprises the following steps: 1) a pre-reaction step; 2) a high temperature reaction step; 3) a leaching step. Optionally, it also comprises a pre-treatment step of the fluorite concentrate; a treatment step of the reaction gas; and a treatment step of the leached residue. The following is a detailed description.

[0030] Pretreatment steps of fluorite concentrate

[0031] The fluorite concentrate is made into balls, and the balls are dried at 90-120°C for 12-36 hours to obtain dried fluorite concentrate particles. This is beneficial to improving the decomposition rate of rare earth and niobium, and further to improving the leaching rate of rare earth and niobium.

[0032] The diameter of the ball can be 2 to 5 mm, preferably 2 to 4 mm, and more preferably 3 to 4 mm. Such a diameter is beneficial to the reaction on the one hand, and is beneficial to the recovery of the fluorite concentrate after drying on the other hand.

[0033] The drying temperature may be 90-120° C., preferably 100-120° C., more preferably 100-110° C. The drying time may be 12-36 hours, preferably 24-36 hours, more preferably 24-30 hours. The moisture content of the dried fluorite concentrate particles is less than 0.1wt%.

[0034] The CaF2 content in the fluorite concentrate is greater than 75wt%, preferably greater than or equal to 80wt%, the REO content can be 5.02-9wt%, preferably 5.04-8wt%, and the Nb2O5 content can be 0.05-0.5wt%, preferably 0.08-0.4wt%. Fluorite concentrate with such content can have a higher rare earth and niobium leaching rate when processed within the specific process and process parameter range of the present invention.

[0035] In the present invention, the rare earth minerals in the fluorite concentrate are mainly one or more of fluorocarbon cerium ore, fluorocarbon calcium cerium ore and Yellow River ore, and the niobium minerals in the fluorite concentrate are mainly one or more of columbite, calcite and niobium rutile.

[0036] Pre-reaction step

[0037] The dried fluorite concentrate particles are mixed with sulfuric acid and pre-reacted at 90-150°C to obtain a pre-reaction material. This is beneficial to improving the decomposition rate of rare earth and niobium, thereby improving the leaching rate of rare earth and niobium.

[0038] The CaF2 content in the dried fluorite concentrate particles is greater than 75wt%, preferably greater than or equal to 80wt%, more preferably greater than or equal to 85wt% and less than 95wt%; the REO content can be 5.02~9wt%, preferably 5.04~8wt%, more preferably 5.2~7.5wt%; the Nb2O5 content can be 0.05~0.5wt%, preferably 0.08~0.4wt%, more preferably 0.1~0.2wt%.

[0039] In the present invention, sulfuric acid is a mixture of 98wt% concentrated sulfuric acid and 105wt% oleum. The mass ratio of the dried fluorite concentrate particles, 98wt% concentrated sulfuric acid and 105wt% oleum can be 1:(0.7-0.9):(0.6-0.8), preferably 1:(0.75-0.9):(0.65-0.8), more preferably 1:(0.8-0.9):(0.7-0.8). According to a specific embodiment of the present invention, the mass ratio of the three is 1:0.9:0.8.

[0040] The pre-reaction temperature may be 90 to 150° C., preferably 100 to 140° C., more preferably 100 to 130° C., and even more preferably 110 to 120° C. The pre-reaction time may be 4 to 10 min, preferably 4 to 8 min, and more preferably 5 to 6 min.

[0041] High temperature reaction step

[0042] The pre-reaction material is reacted at 190-280°C to obtain reaction gas and reaction slag. This is beneficial to improving the decomposition rate of rare earth and niobium, and further to improving the leaching rate of rare earth and niobium. In addition, it is also beneficial to obtain a higher yield of hydrogen fluoride gas.

[0043] The reaction temperature may be 190 to 280° C., preferably 220 to 260° C., more preferably 230 to 250° C. The reaction time may be 55 to 110 min, preferably 60 to 100 min, more preferably 80 to 90 min.

[0044] According to one embodiment of the present invention, the pre-reaction material is reacted at 210-280° C. for 55-110 min to obtain a reaction gas containing hydrogen fluoride and reaction slag.

[0045] In the present invention, the reaction slag is a solid containing rare earth elements, niobium elements and calcium sulfate. The reaction gas is a gas containing hydrogen fluoride.

[0046] Reaction gas processing steps

[0047] In the present invention, the reaction gas containing hydrogen fluoride can be washed by a washing tower, and then condensed and distilled to obtain anhydrous hydrogen fluoride. The recovered acid after washing can be returned to the raw material (dried fluorite concentrate particles) to continue to participate in the reaction, which is conducive to the recycling of the acid.

[0048] Leaching step

[0049] The reaction slag is leached with water to obtain a leaching solution containing rare earth and niobium and a leaching slag.

[0050] The mass ratio of water to reaction slag is 0.14-0.25:1, preferably 0.15-0.22:1, more preferably 0.18-0.21:1, and even more preferably 0.19-0.2:1. This is conducive to improving the leaching rate of rare earth and niobium and improving the purity of rare earth and niobium. In the present invention, the mass of the reaction slag is calculated based on the dry weight of the reaction slag. The present invention has found through research and experiments that the mass ratio of water to reaction slag needs to be controlled within a specific range, otherwise, a higher leaching rate of rare earth and niobium cannot be obtained.

[0051] In the present invention, the leaching rate of rare earth is greater than or equal to 98.5%, preferably greater than or equal to 98.6%, more preferably greater than or equal to 98.9%. The leaching rate of rare earth can reach 99.3%. The leaching rate of niobium is greater than or equal to 85%, preferably greater than or equal to 86%, more preferably greater than or equal to 88%.

[0052] The calculation formula for the leaching rate of rare earth and niobium is as follows:

[0053] The leaching rate of rare earth = 100% - (mass of leached residue × REO content in leached residue / mass of fluorite concentrate × REO content in fluorite concentrate) × 100%.

[0054] The leaching rate of niobium = 100% - (mass of leached slag × content of Nb2O5 in the leached slag / mass of fluorite concentrate × content of Nb2O5 in the fluorite concentrate) × 100%.

[0055] The present invention can adopt an intelligent high-efficiency filter press to perform one-step leaching and filtering to obtain a leaching solution and leaching residue containing rare earth and niobium.

[0056] In the present invention, the leaching solution containing rare earth and niobium can be neutralized and impurities removed by using magnesium oxide to obtain a neutralized leaching solution containing rare earth and niobium and a neutralized slag. The neutralization step can be performed by those known in the art and will not be described in detail herein. The neutralized slag can be returned to the water leaching step for further leaching to recover the residual rare earth and niobium.

[0057] Treatment steps of leaching residue

[0058] The obtained leaching residue is subjected to magnetic separation by a magnetic separator to obtain calcium sulfate, so that gypsum that meets actual needs can be obtained.

[0059] The magnetic separation intensity is 3.5 to 4.5 T, preferably 3.5 to 4.2 T, and more preferably 3.5 to 4.0 T. The purity of the obtained calcium sulfate is greater than or equal to 90 wt%.

[0060] <Analysis Method>

[0061] The analytical test methods used in the embodiments and comparative examples are described below:

[0062] CaF2 content: tested by EDTA (ethylenediaminetetraacetic acid) volumetric method according to standard GB5195.1-85.

[0063] REO content: tested by weight method according to standard GB / T 6730.25-2021.

[0064] Nb2O5 content: tested by weight method, according to standard GB / T 3654.1-1983.

[0065] Purity of gypsum: tested by barium sulfate precipitation method, according to standard GB / T5484-2012.

[0066] Example 1

[0067] In the fluorite concentrate used in this embodiment, the CaF2 content is 88.96wt%, the REO content is 5.68wt%, and the Nb2O5 content is 0.11wt%.

[0068] The fluorite concentrate is made into balls on a disc granulator, the diameter of the balls is 2 to 5 mm, and the prepared balls are dried at 100° C. for 24 hours to obtain dried fluorite concentrate particles.

[0069] The dried fluorite concentrate particles, 98wt% concentrated sulfuric acid and 105wt% oleum are uniformly mixed in a pre-reactor at a mass ratio of 1:0.9:0.8, and reacted rapidly at 120°C for 4 minutes to obtain a pre-reaction material.

[0070] The pre-reaction material is fully reacted at 250° C. for 60 minutes to obtain reaction gas and reaction slag containing hydrogen fluoride. The reactor body containing hydrogen fluoride is passed into a washing tower for washing, condensation and rectification to obtain anhydrous hydrogen fluoride.

[0071] The reaction slag is subjected to one-step leaching and filtration using water using an intelligent high-efficiency filter press to obtain a leaching solution containing rare earth and niobium and a leaching slag, wherein during leaching, the mass ratio of water to reaction slag is 0.2:1.

[0072] The leaching solution containing rare earth and niobium is neutralized and impurities are removed by using magnesium oxide to obtain the neutralized leaching solution containing rare earth and niobium and neutralized slag, wherein the amount of magnesium oxide used is 5.7wt% of the mass of the fluorite concentrate.

[0073] The leached residue was removed from the impurities such as iron and thorium by a superconducting strong magnetic separator, and gypsum (i.e. calcium sulfate) with a high purity was obtained. The magnetic field strength was 4.0 T. The results are shown in Table 2.

[0074] Example 2

[0075] In the fluorite concentrate used in this embodiment, the CaF2 content is 92.16wt%, the REO content is 5.04wt%, and the Nb2O5 content is 0.12wt%.

[0076] The fluorite concentrate is made into balls on a disc granulator, the diameter of the balls is 2 to 5 mm, and the prepared balls are dried at 100° C. for 24 hours to obtain dried fluorite concentrate particles.

[0077] The dried fluorite concentrate particles, 98wt% concentrated sulfuric acid and 105wt% oleum are uniformly mixed in a pre-reactor at a mass ratio of 1:0.7:0.8, and reacted rapidly at 120°C for 5 minutes to obtain a pre-reaction material.

[0078] The pre-reaction material is fully reacted at 240° C. for 80 minutes to obtain reaction gas and reaction slag containing hydrogen fluoride. The reactor body containing hydrogen fluoride is passed into a washing tower for washing, condensation and rectification to obtain anhydrous hydrogen fluoride.

[0079] The reaction slag is subjected to one-step leaching and filtration using water using an intelligent high-efficiency filter press to obtain a leaching solution containing rare earth and niobium and a leaching slag, wherein during leaching, the mass ratio of water to reaction slag is 0.15:1.

[0080] The leaching solution containing rare earth and niobium is neutralized and impurities are removed by using magnesium oxide to obtain the neutralized leaching solution containing rare earth and niobium and neutralized slag, wherein the amount of magnesium oxide used is 5.05wt% of the mass of the fluorite concentrate.

[0081] The leached residue was removed from the impurities such as iron and thorium by a superconducting strong magnetic separator, and gypsum with a high purity was obtained. The magnetic field strength was 4.0 T. The results are shown in Table 2.

[0082] Example 3

[0083] In the fluorite concentrate used in this embodiment, the CaF2 content is 82.64wt%, the REO content is 6.41wt%, and the Nb2O5 content is 0.12wt%.

[0084] The fluorite concentrate is made into balls on a disc granulator, the diameter of the balls is 2 to 5 mm, and the prepared balls are dried at 100° C. for 24 hours to obtain dried fluorite concentrate particles.

[0085] The dried fluorite concentrate particles, 98wt% concentrated sulfuric acid and 105wt% oleum are uniformly mixed in a pre-reactor at a mass ratio of 1:0.8:0.8, and reacted rapidly at 100°C for 6 minutes to obtain a pre-reaction material.

[0086] The pre-reaction material is fully reacted at 230° C. for 90 minutes to obtain reaction gas and reaction residue containing hydrogen fluoride. The reactor body containing hydrogen fluoride is passed into a washing tower for washing, condensation and rectification to obtain anhydrous hydrogen fluoride.

[0087] The reaction slag is subjected to one-step leaching and filtration using water in an intelligent high-efficiency filter press to obtain a leaching solution containing rare earth and niobium and a leaching slag, wherein during leaching, the mass ratio of water to reaction slag is 0.14:1.

[0088] The leaching solution containing rare earth and niobium is neutralized and impurities are removed by using magnesium oxide to obtain the neutralized leaching solution containing rare earth and niobium and neutralized slag, wherein the amount of magnesium oxide used is 6.5wt% of the mass of the fluorite concentrate.

[0089] The leached residue was removed from the impurities such as iron and thorium by a superconducting strong magnetic separator, and gypsum with a high purity was obtained. The magnetic field strength was 3.5 T. The results are shown in Table 2.

[0090] Comparative Example 1

[0091] The difference from Example 1 is that in step 3), during leaching, the mass ratio of water to reaction residue is 0.09:1.

[0092] Comparative Example 2

[0093] The difference from Example 1 is that the mass ratio of the dried fluorite concentrate particles, 98 wt % concentrated sulfuric acid and 105 wt % oleum is 1:0.5:0.9.

[0094] Table 1

[0095]

[0096] Note: In Table 1, M refers to the mass ratio of dried fluorite concentrate particles, 98% concentrated sulfuric acid, and 105% oleum; N refers to the mass ratio of water to reaction slag during leaching.

[0097] Table 2

[0098] serial number Leaching rate of rare earth % Niobium leaching rate % Purity of gypsum % Example 1 99.3 88.6 90.3 Example 2 98.9 86.8 94.0 Example 3 98.6 86.9 90.4 Comparative Example 1 95.3 83.2 89.2 Comparative Example 2 96.4 82.9 89.8

[0099] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.

Claims

1. A method for recovering rare earth and niobium from fluorite concentrate, It is characterized in that The steps include: 1) The fluorite concentrate is made into balls with a diameter of 2 to 5 mm, and the prepared balls are dried at 90 to 120° C. for 12 to 36 hours to obtain dried fluorite concentrate particles; the dried fluorite concentrate particles are mixed with sulfuric acid, and pre-reacted at 100 to 120° C. for 4 to 8 minutes to obtain a pre-reaction material; 2) reacting the pre-reaction material at 220-260° C. for 60-110 min to obtain reaction gas and reaction slag; 3) leaching the reaction slag with water to obtain a leaching solution containing rare earth and niobium and a leaching slag; Among them, CaF 2 The content is greater than 75wt%, the REO content is 5.02-9wt%, and the Nb 2 O 5 The content is 0.05-0.5wt%; the rare earth minerals in the fluorite concentrate are mainly one or more of fluorocarbon cerium ore, fluorocarbon calcium cerium ore and Yellow River ore, and the niobium minerals in the fluorite concentrate are mainly one or more of columbite, calcite and niobium iron rutile; Wherein, the sulfuric acid is a mixture of 98wt% concentrated sulfuric acid and 105wt% oleum; the mass ratio of the dried fluorite concentrate particles, 98wt% concentrated sulfuric acid and 105wt% oleum is 1:(0.7-0.9):(0.6-0.8); Among them, the mass ratio of water to reaction slag is 0.14-0.22:1; The leaching rate of rare earth is greater than or equal to 98.6%, and the leaching rate of niobium is greater than or equal to 86%.

2. The method according to claim 1, It is characterized in that In step 2), the reaction time is 60 to 100 minutes.

3. The method according to claim 1, It is characterized in that The method also includes the following steps: washing the reaction gas containing hydrogen fluoride through a washing tower, and then condensing and rectifying to obtain anhydrous hydrogen fluoride.

4. The method according to claim 1, It is characterized in that In step 3), the mass ratio of water to reaction slag is 0.15-0.22:

1.

5. The method according to claim 1, It is characterized in that The following steps are also included: The leaching solution containing rare earth and niobium obtained in step 3) is neutralized with magnesium oxide to obtain a neutralized leaching solution containing rare earth and niobium and a neutralized slag; The leached residue obtained in step 3) is subjected to magnetic separation by a magnetic separator to obtain calcium sulfate; wherein the magnetic separation intensity is 3.5 to 4.5 T; and the purity of the obtained calcium sulfate is greater than or equal to 90 wt%.

Citation Information

Patent Citations

  • Method for comprehensively recovering fluorine and tungsten from tungsten-containing fluorite mineral

    CN102925670A

  • Method for treating rare-earth-containing low-grade fluorite minerals

    CN109371239A

  • Method for preparing hydrogen fluoride by recovering fluorite with rare earth

    CN113735062A

  • Method for producing alumina by using pulverized fuel ash

    CN102502729A

  • Method for using low-grade niobium concentrate to produce niobium-iron alloy and rare earth double sulfate salt

    CN104894363A