A hot-dip galvanizing solution with alloy added

By adding alloy elements such as Al, Ni, Zr, Sc, Pr, Bi, Re to the hot-dip galvanizing solution to form a plating layer, the problem of insufficient adhesion and corrosion resistance of the plating layer in the prior art is solved, and uniform plating layer is achieved Significant improvement in properties and corrosion resistance.

CN115852288BActive Publication Date: 2024-11-01JIANGSU POWER EQUIP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211697743.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-28
Publication Date
2024-11-01
Estimated Expiration
2042-12-28

AI Technical Summary

Technical Problem

The existing hot-dip galvanizing technology has shortcomings in improving the adhesion and corrosion resistance of the coating, especially in special environments such as electric towers, the performance of the coating is difficult to meet the long-term exposure usage requirements.

Method used

Hot-dip galvanizing solution with added alloy was used, with contents of Al: 0.025-0.030%, Ni: 0.005-0.009%, Zr: 0.0002-0.0003%, Sc: 0.0006-0.0009%, Pr: 0.002-0.003%, Bi: 0.004- 0.010%, Re: 0.001-0.005%, the balance is Zn and inevitable impurities. By smelting the multi-alloy and dissolving it evenly in the zinc liquid, forming a plating layer.

Benefits of technology

Significantly improve the structure of the plating layer, thin the thickness of the plating layer, improve the uniformity and corrosion resistance of the plating layer, enhance the corrosion resistance of the plating layer, and meet the corrosion protection requirements of structural parts such as power towers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004024104090000141
    Figure BDA0004024104090000141
Patent Text Reader

Abstract

The invention provides a hot-dip galvanizing solution with alloy addition, which comprises the following alloy element components in mass percentage: Al: 0.025-0.030%; Ni: 0.005%-0.009%; Zr: 0.0002-0.0003%; Sc: 0.0006-0.0009%; Pr: 0.002-0.003%; Bi: 0.004-0010%; Re: 0.001-0.005%; and the balance is Zn and unavoidable impurities.
Need to check novelty before this filing date? Find Prior Art

Description

Field of the Invention

[0001] The invention relates to the field of steel surface corrosion protection, and in particular to an alloy-added hot-dip galvanizing solution and a preparation method thereof. Background of the Invention

[0002] Hot-dip galvanizing technology is one of the effective methods to improve the atmospheric corrosion resistance of steel. Hot-dip galvanizing products are widely used in the fields of electricity, transportation, communication, construction, home appliances, etc., such as highway guardrails, ultra-high voltage transmission towers, communication towers, building steel structures, etc. According to different process methods, hot-dip galvanizing can be divided into continuous galvanizing and batch galvanizing. Continuous hot-dip galvanizing is to immerse continuous steel into a zinc bath at high speed through a hot galvanizing unit for plating, and the coating needs to be blown; batch hot-dip galvanizing is to immerse the processed steel components in a zinc bath for plating in a single piece or batch, and the coating does not need to be blown. Its main process flow includes: alkaline washing and degreasing, water washing, pickling and rust removal, water washing, solvent immersion plating, hot-dip galvanizing, quenching and cooling, and passivation. People have always solved the problem of hot-dip galvanizing by adding alloy elements to the zinc bath to improve the fluidity and adhesion of zinc, and improve the corrosion resistance of the coating and the formability of the plated parts, such as adding Al, Ni, Mg, Sb, RE and other elements to the zinc bath. With the diversified development of hot-dip galvanized products, higher requirements are placed on their performance, especially for power towers, which are exposed for a long time, especially in some special use environments, it is necessary to further improve the adhesion and corrosion resistance of the galvanized layer. Therefore, it is urgent to develop various high-performance hot-dip galvanized alloy coatings. Summary of the invention

[0003] The invention provides an alloy-added hot-dip galvanizing solution, which comprises the following alloy element components in mass percentage: Al: 0.025-0.030%; Ni: 0.005%-0.009%; Zr: 0.0002-0.0003%; Sc: 0.0006-0.0009%; Pr: 0.002-0.003%; Bi: 0.004-0010%; Re: 0.001-0.005%; the balance is Zn and unavoidable impurities.

[0004] Preferably, the ratio of Sc / Zr in the alloy-added hot-dip galvanizing solution is 3 / 1.

[0005] Preferably, the alloy-added hot-dip galvanizing liquid contains the following alloy element components in mass percentage: Al: 0.025-0.030%; Ni: 0.005%-0.009%; Zr: 0.0002%; Sc: 0.0006%; Pr: 0.002-0.003%; Bi: 0.004-0010%; Re: 0.001-0.005%; the balance is Zn and unavoidable impurities.

[0006] Preferably, the alloy-added hot-dip galvanizing liquid contains the following alloy element components in mass percentage: Al: 0.025-0.030%; Ni: 0.005%-0.009%; Zr: 0.0003%; Sc: 0.0009%; Pr: 0.002-0.003%; Bi: 0.004-0010%; Re: 0.001-0.005%; the balance is Zn and unavoidable impurities.

[0007] Preferably, the alloy-added hot-dip galvanizing solution of the present invention is suitable for batch hot-dip galvanizing of power tower components.

[0008] The present invention also provides a method for preparing the alloy-added hot-dip galvanizing solution of the present invention, which comprises:

[0009] 1) melting Al raw material, Ni raw material, Zr raw material, Sc raw material, Pr raw material, Bi raw material, Re raw material and Zn raw material with good proportion to prepare a multi-element alloy;

[0010] 2) placing the multi-component alloy prepared in step 1) in a stone square cage, immersing it in molten zinc liquid, and moving it back and forth in the zinc pot until the multi-component alloy is completely melted, so that the alloy element components are evenly dissolved in the zinc liquid, thereby preparing a hot-dip galvanizing liquid with added alloy;

[0011] The alloy-added hot-dip galvanizing solution contains the following alloy element components in mass percentage: Al: 0.025-0.030%; Ni: 0.005%-0.009%; Zr: 0.0002-0.0004%; Sc: 0.0006-0.0009%; Pr: 0.002-0.003%; Bi: 0.004-0010%; Re: 0.001-0.005%; the balance is Zn and unavoidable impurities.

[0012] Preferably, the ratio of Sc / Zr in the alloy-added hot-dip galvanizing solution is 3 / 1.

[0013] Preferably, the alloy-added hot-dip galvanizing liquid contains the following alloy element components in mass percentage: Al: 0.025-0.030%; Ni: 0.005%-0.009%; Zr: 0.0002%; Sc: 0.0006%; Pr: 0.002-0.003%; Bi: 0.004-0010%; Re: 0.001-0.005%; the balance is Zn and unavoidable impurities.

[0014] Preferably, the alloy-added hot-dip galvanizing liquid contains the following alloy element components in mass percentage: Al: 0.025-0.030%; Ni: 0.005%-0.009%; Zr: 0.0003%; Sc: 0.0009%; Pr: 0.002-0.003%; Bi: 0.004-0010%; Re: 0.001-0.005%; the balance is Zn and unavoidable impurities.

[0015] Preferably, the alloy-added hot-dip galvanizing solution is suitable for batch hot-dip galvanizing of power tower components.

[0016] The present invention also provides a hot-dip galvanizing method, which comprises placing a substrate to be plated in the alloy-added hot-dip galvanizing solution of the present invention to form a coating on the surface of the substrate to be plated.

[0017] Preferably, the substrate to be plated includes various angle steels, connecting plates and welded parts.

[0018] In an exemplary embodiment, the hot-dip galvanizing method may include the following steps:

[0019] 1) Pre-treat the substrate to be plated, including degreasing, pickling, immersion in plating agent and drying;

[0020] 2) immersing the pretreated substrate to be plated into a molten hot-dip galvanizing solution containing an alloy added according to the present invention to form a coating on the surface of the substrate to be plated;

[0021] 3) Surface finishing of the coating;

[0022] 4) Cooling and inspection.

[0023] In an exemplary embodiment, the working concentration of the plating aid is 80-100 g / L, the temperature is 60-80° C., the immersion time is 40-60 s, the pH value of the plating aid is 5-6, and it includes 30-40% zinc chloride, 25-35% ammonium chloride, 1-5% rare earth chloride and 30-50% water by mass percentage.

[0024] Beneficial effects of the present invention

[0025] In the alloy-added hot-dip galvanizing solution of the present invention, the content of Al is 0.025-0.030% (unless otherwise specified, the percentages in this specification are all mass percentages). For example, the content of Al is 0.025%, 0.026%, 0.027%, 0.028%, 0.029%, 0.030% or any range between the aforementioned values. In the galvanizing solution, Al first reacts with iron to form an Al-Fe phase, which has a significant inhibitory effect on the growth of the iron-zinc alloy layer, and can well improve the structure of the coating and thin the coating. If the content of Al is lower than 0.025%, the thinning effect of the coating and the improvement of corrosion resistance are both worse. If the content of Al is higher than 0.030%, the hot-dip galvanized layer is greatly thinned due to the effect of more aluminum in the hot-dip galvanizing solution, and its thickness cannot meet the corrosion protection requirements of structural parts.

[0026] In the alloy-added hot-dip galvanizing solution of the present invention, the content of Ni is 0.005%-0.009%. For example, the content of Ni is 0.005%, 0.006%, 0.007%, 0.008%, 0.009% or any range between the aforementioned values. The addition of Ni can inhibit the growth of the steel coating on the one hand, and on the other hand, it can improve the fluidity of the hot-dip galvanizing solution, making the coating uniform and smooth, with appropriate thickness, reducing zinc consumption and reducing costs. If the content of Ni is lower than 0.005%, the inhibition of excessively thick growth of the steel coating is not obvious, and the fluidity of the hot-dip galvanizing solution cannot be effectively improved; if the content of Ni is higher than 0.009%, Fe-Zn-Ni ternary phase slag may be generated, which adheres to the surface of the coating and causes particles to appear on the surface of the plated part.

[0027] In the alloy-added hot-dip galvanizing solution of the present invention, the content of Sc is 0.0006-0.0009%. For example, the content of Sc is 0.0006%, 0.0007%, 0.0008%, 0.0009% or any range between the aforementioned values. In the alloy-added hot-dip galvanizing solution of the present invention, the content of Zr is 0.0002-0.0003%. For example, the content of Zr is 0.0002%, 0.00023%, 0.00027%, 0.0003% or any range between the aforementioned values.

[0028] In the alloy-added hot-dip galvanizing solution of the present invention, Sc and Zr do not form Al with Al. 3 Sc phase and Al 3 Zr phase or Al 3(Sc, Zr) phase, but solid solution in the Al-Fe phase and enriched around the Al-Fe phase, thereby refining the grains of the Al-Fe phase in the alloy structure, improving the plasticity of the coating, and slowing down the growth rate of the Al-Fe phase, improving the uniformity and thickness of the coating. The inventors have found that when the ratio of Sc to Zr is 3:1, the improvement effect of Sc and Zr is significantly improved, and the improvement effect is not as good above or below this ratio. If the content of Sc and Zr is lower than the range specified in the present invention, Sc and Zr cannot fully play the role of refining the grains and slowing down the growth rate of the Al-Fe phase; if the content of Sc and Zr is higher than the range specified in the present invention, Sc and Zr will form Al with Al. 3 Sc phase and Al 3 Zr phase or Al 3 (Sc, Zr) phase, thus affecting the formation of Al-Fe phase, which is not conducive to the thinning of the coating, and cannot play the function of refining the grains and slowing down the growth rate of the Al-Fe phase.

[0029] In the alloy-added hot-dip galvanizing liquid of the present invention, the content of Pr is 0.002-0.003%. For example, the content of Pr is 0.002%, 0.0025%, 0.003% or any range between the aforementioned values. On the one hand, it can protect the coating from oxidation, and on the other hand, it can form a Fe-Zn-Pr phase with Fe and Zn, and refine the iron-zinc alloy structure through the eutectic reaction, thereby obtaining an alloy layer with fine grains and thin thickness. If the amount of Pr is too low, the effect is not significant. If the amount of Pr is too high, Pr will precipitate from the liquid, thereby adhering to the surface of the coating and causing particles to appear on the surface of the plated part.

[0030] In the alloy-added hot-dip galvanizing solution of the present invention, Bi and Re improve the fluidity of the zinc solution, improve the generation of droplets and burrs, and enhance the corrosion resistance of the zinc layer. Example

[0031] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0032] Embodiment 1:

[0033] This embodiment provides a hot-dip galvanizing solution with alloy addition and a preparation method thereof, which comprises

[0034] 1) melting Al raw material, Ni raw material, Zr raw material, Sc raw material, Pr raw material, Bi raw material, Re raw material and Zn raw material with good proportion to prepare a multi-element alloy;

[0035] 2) placing the multi-component alloy prepared in step 1) in a stone square cage, immersing it in molten zinc liquid, and moving it back and forth in the zinc pot until the multi-component alloy is completely melted, so that the alloy element components are evenly dissolved in the zinc liquid, thereby preparing a hot-dip galvanizing liquid with added alloy;

[0036] The alloy-added hot-dip galvanizing solution contains the following alloy element components in mass percentage: Al: 0.025%; Ni: 0.005%; Zr: 0.0002%; Sc: 0.0006%; Pr: 0.0025%; Bi: 0.004%; Re: 0.001%; ​​the remainder is Zn and unavoidable impurities.

[0037] Using the alloy-added hot-dip galvanizing solution prepared in this embodiment to perform hot-dip galvanizing on a substrate to be plated includes the following steps:

[0038] 1) Immerse the Q235 steel plate parts (10cm×5cm×2mm) in a NaOH solution with a mass percentage concentration of 10% for alkaline washing and degreasing treatment. The alkaline washing temperature is 70℃ and the alkaline washing time is 10min. After taking out, rinse the surface with clean water. Then immerse the steel plate parts after alkaline washing and degreasing in a HCl pickling solution with a mass percentage concentration of 10% for pickling and rust removal. The pickling temperature is 25℃ and the pickling time is 20min. After taking out, rinse with clean water. Finally, immerse the steel plate parts after pickling in 100g / L plating aid for plating. The composition of the plating aid is: 40% zinc chloride, 25% ammonium chloride, 1% rare earth chloride and 34% water in mass volume percentage. The plating temperature is 60℃ and the plating time is 60s;

[0039] 2) immersing the pretreated steel plate product into a molten hot-dip galvanizing solution with an alloy added according to this embodiment, with a galvanizing temperature of 450° C. and a galvanizing time of 60 seconds to form a coating on the surface of the steel plate product;

[0040] 3) Surface finishing of the coating;

[0041] 4) Cooling and inspection.

[0042] The thickness of the batch hot-dip galvanized coating obtained in this embodiment was tested by a magnetic thickness gauge, and a salt spray corrosion resistance test was performed. After removing the corrosion products of the batch hot-dip galvanized coating, the average corrosion weight loss change within 15 neutral salt spray test cycles was statistically analyzed to obtain the average corrosion rate. The results are shown in Table 1.

[0043] Embodiment 2:

[0044] This embodiment provides a hot-dip galvanizing solution with alloy addition and a preparation method thereof, which comprises

[0045] 1) melting Al raw material, Ni raw material, Zr raw material, Sc raw material, Pr raw material, Bi raw material, Re raw material and Zn raw material with good proportion to prepare a multi-element alloy;

[0046] 2) placing the multi-component alloy prepared in step 1) in a stone square cage, immersing it in molten zinc liquid, and moving it back and forth in the zinc pot until the multi-component alloy is completely melted, so that the alloy element components are evenly dissolved in the zinc liquid, thereby preparing a hot-dip galvanizing liquid with added alloy;

[0047] The alloy-added hot-dip galvanizing solution contains the following alloy element components in mass percentage: Al: 0.03%; Ni: 0.007%; Zr: 0.0002%; Sc: 0.0006%; Pr: 0.0020%; Bi: 0.006%; Re: 0.003%; the remainder is Zn and unavoidable impurities.

[0048] As described in Example 1, the hot-dip galvanizing liquid with alloy added prepared in this example is used to perform hot-dip galvanizing on the substrate to be plated.

[0049] The thickness of the batch hot-dip galvanized coating obtained in this embodiment was tested by a magnetic thickness gauge, and a salt spray corrosion resistance test was performed. After removing the corrosion products of the batch hot-dip galvanized coating, the average corrosion weight loss change within 15 neutral salt spray test cycles was statistically analyzed to obtain the average corrosion rate. The results are shown in Table 1.

[0050] Embodiment 3:

[0051] This embodiment provides a hot-dip galvanizing solution with alloy addition and a preparation method thereof, which comprises

[0052] 1) melting Al raw material, Ni raw material, Zr raw material, Sc raw material, Pr raw material, Bi raw material, Re raw material and Zn raw material with good proportion to prepare a multi-element alloy;

[0053] 2) placing the multi-component alloy prepared in step 1) in a stone square cage, immersing it in molten zinc liquid, and moving it back and forth in the zinc pot until the multi-component alloy is completely melted, so that the alloy element components are evenly dissolved in the zinc liquid, thereby preparing a hot-dip galvanizing liquid with added alloy;

[0054] The alloy-added hot-dip galvanizing solution contains the following alloy element components in mass percentage: Al: 0.03%; Ni: 0.008%; Zr: 0.00027%; Sc: 0.0008%; Pr: 0.0025%; Bi: 0.010%; Re: 0.005%; the remainder is Zn and unavoidable impurities.

[0055] As described in Example 1, the hot-dip galvanizing liquid with alloy added prepared in this example is used to perform hot-dip galvanizing on the substrate to be plated.

[0056] The thickness of the batch hot-dip galvanized coating obtained in this embodiment was tested by a magnetic thickness gauge, and a salt spray corrosion resistance test was performed. After removing the corrosion products of the batch hot-dip galvanized coating, the average corrosion weight loss change within 15 neutral salt spray test cycles was statistically analyzed to obtain the average corrosion rate. The results are shown in Table 1.

[0057] Embodiment 4:

[0058] This embodiment provides a hot-dip galvanizing solution with alloy addition and a preparation method thereof, which comprises

[0059] 1) melting Al raw material, Ni raw material, Zr raw material, Sc raw material, Pr raw material, Bi raw material, Re raw material and Zn raw material with good proportion to prepare a multi-element alloy;

[0060] 2) placing the multi-component alloy prepared in step 1) in a stone square cage, immersing it in molten zinc liquid, and moving it back and forth in the zinc pot until the multi-component alloy is completely melted, so that the alloy element components are evenly dissolved in the zinc liquid, thereby preparing a hot-dip galvanizing liquid with added alloy;

[0061] The alloy-added hot-dip galvanizing solution contains the following alloy element components in mass percentage: Al: 0.03%; Ni: 0.007%; Zr: 0.0003%; Sc: 0.0009%; Pr: 0.0025%; Bi: 0.006%; Re: 0.003%; the remainder is Zn and unavoidable impurities.

[0062] As described in Example 1, the hot-dip galvanizing liquid with alloy added prepared in this example is used to perform hot-dip galvanizing on the substrate to be plated.

[0063] The thickness of the batch hot-dip galvanized coating obtained in this embodiment was tested by a magnetic thickness gauge, and a salt spray corrosion resistance test was performed. After removing the corrosion products of the batch hot-dip galvanized coating, the average corrosion weight loss change within 15 neutral salt spray test cycles was statistically analyzed to obtain the average corrosion rate. The results are shown in Table 1.

[0064] Embodiment 5:

[0065] This embodiment provides a hot-dip galvanizing solution with alloy addition and a preparation method thereof, which comprises

[0066] 1) melting Al raw material, Ni raw material, Zr raw material, Sc raw material, Pr raw material, Bi raw material, Re raw material and Zn raw material with good proportion to prepare a multi-element alloy;

[0067] 2) placing the multi-component alloy prepared in step 1) in a stone square cage, immersing it in molten zinc liquid, and moving it back and forth in the zinc pot until the multi-component alloy is completely melted, so that the alloy element components are evenly dissolved in the zinc liquid, thereby preparing a hot-dip galvanizing liquid with added alloy;

[0068] The alloy-added hot-dip galvanizing solution contains the following alloy element components in mass percentage: Al: 0.03%; Ni: 0.009%; Zr: 0.0003%; Sc: 0.0009%; Pr: 0.003%; Bi: 0.010%; Re: 0.005%; the remainder is Zn and unavoidable impurities.

[0069] As described in Example 1, the hot-dip galvanizing liquid with alloy added prepared in this example is used to perform hot-dip galvanizing on the substrate to be plated.

[0070] The thickness of the batch hot-dip galvanized coating obtained in this embodiment was tested by a magnetic thickness gauge, and a salt spray corrosion resistance test was performed. After removing the corrosion products of the batch hot-dip galvanized coating, the average corrosion weight loss change within 15 neutral salt spray test cycles was statistically analyzed to obtain the average corrosion rate. The results are shown in Table 1.

[0071] Comparative Example 1

[0072] Hot-dip galvanizing of the substrate to be plated using hot-dip pure zinc liquid includes the following steps:

[0073] 1) Immerse the Q235 steel plate parts (10cm×5cm×2mm) in a NaOH solution with a mass percentage concentration of 10% for alkaline washing and degreasing treatment. The alkaline washing temperature is 70℃ and the alkaline washing time is 10min. After taking out, rinse the surface with clean water. Then immerse the steel plate parts after alkaline washing and degreasing in a HCl pickling solution with a mass percentage concentration of 10% for pickling and rust removal. The pickling temperature is 25℃ and the pickling time is 20min. After taking out, rinse with clean water. Finally, immerse the steel plate parts after pickling in 100g / L plating aid for plating. The composition of the plating aid is: 40% zinc chloride, 25% ammonium chloride, 1% rare earth chloride and 34% water in mass volume percentage. The plating temperature is 60℃ and the plating time is 60s;

[0074] 2) immersing the pretreated steel plate into a pure Zn bath at a galvanizing temperature of 450° C. for 60 seconds to form a pure Zn coating on the surface of the steel plate;

[0075] 3) Surface finishing of the coating;

[0076] 4) Cooling and inspection.

[0077] The thickness of the pure Zn coating obtained in this comparative example was tested by a magnetic thickness gauge, and a salt spray corrosion resistance test was performed. After removing the corrosion products of the batch hot-dip galvanized coating, the average corrosion weight loss change within 15 neutral salt spray test cycles was statistically analyzed to obtain the average corrosion rate. The results are shown in Table 1.

[0078] Comparative Example 2:

[0079] This comparative example provides a hot-dip galvanizing solution with alloy addition and a preparation method thereof, which comprises

[0080] 1) melting Al raw material, Ni raw material, Pr raw material, Bi raw material, Re raw material and Zn raw material with good proportion to prepare a multi-element alloy;

[0081] 2) placing the multi-component alloy prepared in step 1) in a stone square cage, immersing it in molten zinc liquid, and moving it back and forth in the zinc pot until the multi-component alloy is completely melted, so that the alloy element components are evenly dissolved in the zinc liquid, thereby preparing a hot-dip galvanizing liquid with added alloy;

[0082] The alloy-added hot-dip galvanizing solution contains the following alloy element components in mass percentage: Al: 0.03%; Ni: 0.008%; Pr: 0.0025%; Bi: 0.010%; Re: 0.005%; the remainder is Zn and unavoidable impurities.

[0083] As described in Example 1, the hot-dip galvanizing liquid with alloy added prepared in this comparative example was used to perform hot-dip galvanizing on the substrate to be plated.

[0084] The thickness of the batch hot-dip galvanized coating obtained in this comparative example was tested by a magnetic thickness gauge, and a salt spray corrosion resistance test was performed. After removing the corrosion products of the batch hot-dip galvanized coating, the average corrosion weight loss change within 15 neutral salt spray test cycles was statistically analyzed to obtain the average corrosion rate. The results are shown in Table 1.

[0085] Comparative Example 3:

[0086] This comparative example provides a hot-dip galvanizing solution with alloy addition and a preparation method thereof, which comprises

[0087] 1) melting Al raw material, Ni raw material, Zr raw material, Pr raw material, Bi raw material, Re raw material and Zn raw material with good proportion to prepare a multi-element alloy;

[0088] 2) placing the multi-component alloy prepared in step 1) in a stone square cage, immersing it in molten zinc liquid, and moving it back and forth in the zinc pot until the multi-component alloy is completely melted, so that the alloy element components are evenly dissolved in the zinc liquid, thereby preparing a hot-dip galvanizing liquid with added alloy;

[0089] The alloy-added hot-dip galvanizing solution contains the following alloy element components in mass percentage: Al: 0.03%; Ni: 0.008%; Zr: 0.00027%; Pr: 0.0025%; Bi: 0.010%; Re: 0.005%; the remainder is Zn and unavoidable impurities.

[0090] As described in Example 1, the hot-dip galvanizing liquid with alloy added prepared in this comparative example was used to perform hot-dip galvanizing on the substrate to be plated.

[0091] The thickness of the batch hot-dip galvanized coating obtained in this comparative example was tested by a magnetic thickness gauge, and a salt spray corrosion resistance test was performed. After removing the corrosion products of the batch hot-dip galvanized coating, the average corrosion weight loss change within 15 neutral salt spray test cycles was statistically analyzed to obtain the average corrosion rate. The results are shown in Table 1.

[0092] Comparative Example 4:

[0093] This comparative example provides a hot-dip galvanizing solution with alloy addition and a preparation method thereof, which comprises

[0094] 1) melting Al raw material, Ni raw material, Sc raw material, Pr raw material, Bi raw material, Re raw material and Zn raw material with good proportion to prepare a multi-element alloy;

[0095] 2) placing the multi-component alloy prepared in step 1) in a stone square cage, immersing it in molten zinc liquid, and moving it back and forth in the zinc pot until the multi-component alloy is completely melted, so that the alloy element components are evenly dissolved in the zinc liquid, thereby preparing a hot-dip galvanizing liquid with added alloy;

[0096] The alloy-added hot-dip galvanizing solution contains the following alloy element components in mass percentage: Al: 0.03%; Ni: 0.008%; Sc: 0.0008%; Pr: 0.0025%; Bi: 0.010%; Re: 0.005%; the remainder is Zn and unavoidable impurities.

[0097] As described in Example 1, the hot-dip galvanizing liquid with alloy added prepared in this comparative example was used to perform hot-dip galvanizing on the substrate to be plated.

[0098] The thickness of the batch hot-dip galvanized coating obtained in this comparative example was tested by a magnetic thickness gauge, and a salt spray corrosion resistance test was performed. After removing the corrosion products of the batch hot-dip galvanized coating, the average corrosion weight loss change within 15 neutral salt spray test cycles was statistically analyzed to obtain the average corrosion rate. The results are shown in Table 1.

[0099] Comparative Example 5:

[0100] This comparative example provides a hot-dip galvanizing solution with alloy addition and a preparation method thereof, which comprises

[0101] 1) melting Al raw material, Ni raw material, Zr raw material, Sc raw material, Pr raw material, Bi raw material, Re raw material and Zn raw material with good proportion to prepare a multi-element alloy;

[0102] 2) placing the multi-component alloy prepared in step 1) in a stone square cage, immersing it in molten zinc liquid, and moving it back and forth in the zinc pot until the multi-component alloy is completely melted, so that the alloy element components are evenly dissolved in the zinc liquid, thereby preparing a hot-dip galvanizing liquid with added alloy;

[0103] The alloy-added hot-dip galvanizing solution contains the following alloy element components in mass percentage: Al: 0.03%; Ni: 0.008%; Zr: 0.0002%; Sc: 0.0008%; Pr: 0.0025%; Bi: 0.010%; Re: 0.005%; the remainder is Zn and unavoidable impurities.

[0104] As described in Example 1, the hot-dip galvanizing liquid with alloy added prepared in this comparative example was used to perform hot-dip galvanizing on the substrate to be plated.

[0105] The thickness of the batch hot-dip galvanized coating obtained in this comparative example was tested by a magnetic thickness gauge, and a salt spray corrosion resistance test was performed. After removing the corrosion products of the batch hot-dip galvanized coating, the average corrosion weight loss change within 15 neutral salt spray test cycles was statistically analyzed to obtain the average corrosion rate. The results are shown in Table 1.

[0106] Comparative Example 6:

[0107] This comparative example provides a hot-dip galvanizing solution with alloy addition and a preparation method thereof, which comprises

[0108] 1) melting Al raw material, Ni raw material, Zr raw material, Sc raw material, Pr raw material, Bi raw material, Re raw material and Zn raw material with good proportion to prepare a multi-element alloy;

[0109] 2) placing the multi-component alloy prepared in step 1) in a stone square cage, immersing it in molten zinc liquid, and moving it back and forth in the zinc pot until the multi-component alloy is completely melted, so that the alloy element components are evenly dissolved in the zinc liquid, thereby preparing a hot-dip galvanizing liquid with added alloy;

[0110] The alloy-added hot-dip galvanizing solution contains the following alloy element components in mass percentage: Al: 0.03%; Ni: 0.008%; Zr: 0.0003%; Sc: 0.0008%; Pr: 0.0025%; Bi: 0.010%; Re: 0.005%; the remainder is Zn and unavoidable impurities.

[0111] As described in Example 1, the hot-dip galvanizing liquid with alloy added prepared in this comparative example was used to perform hot-dip galvanizing on the substrate to be plated.

[0112] Comparative Example 7:

[0113] This comparative example provides a hot-dip galvanizing solution with alloy addition and a preparation method thereof, which comprises

[0114] 1) melting Al raw material, Ni raw material, Zr raw material, Sc raw material, Pr raw material, Bi raw material, Re raw material and Zn raw material with good proportion to prepare a multi-element alloy;

[0115] 2) placing the multi-component alloy prepared in step 1) in a stone square cage, immersing it in molten zinc liquid, and moving it back and forth in the zinc pot until the multi-component alloy is completely melted, so that the alloy element components are evenly dissolved in the zinc liquid, thereby preparing a hot-dip galvanizing liquid with added alloy;

[0116] The alloy-added hot-dip galvanizing solution contains the following alloy element components in mass percentage: Al: 0.03%; Ni: 0.008%; Zr: 0.00033%; Sc: 0.001%; ​​Pr: 0.0025%; Bi: 0.010%; Re: 0.005%; the remainder is Zn and unavoidable impurities.

[0117] As described in Example 1, the hot-dip galvanizing liquid with alloy added prepared in this comparative example was used to perform hot-dip galvanizing on the substrate to be plated.

[0118] The thickness of the batch hot-dip galvanized coating obtained in this comparative example was tested by a magnetic thickness gauge, and a salt spray corrosion resistance test was performed. After removing the corrosion products of the batch hot-dip galvanized coating, the average corrosion weight loss change within 15 neutral salt spray test cycles was statistically analyzed to obtain the average corrosion rate. The results are shown in Table 1.

[0119] Comparative Example 8:

[0120] This comparative example provides a hot-dip galvanizing solution with alloy addition and a preparation method thereof, which comprises

[0121] 1) melting Al raw material, Ni raw material, Zr raw material, Sc raw material, Pr raw material, Bi raw material, Re raw material and Zn raw material with good proportion to prepare a multi-element alloy;

[0122] 2) placing the multi-component alloy prepared in step 1) in a stone square cage, immersing it in molten zinc liquid, and moving it back and forth in the zinc pot until the multi-component alloy is completely melted, so that the alloy element components are evenly dissolved in the zinc liquid, thereby preparing a hot-dip galvanizing liquid with added alloy;

[0123] The alloy-added hot-dip galvanizing solution contains the following alloy element components in mass percentage: Al: 0.03%; Ni: 0.008%; Zr: 0.00067%; Sc: 0.002%; Pr: 0.0025%; Bi: 0.010%; Re: 0.005%; the remainder is Zn and unavoidable impurities.

[0124] As described in Example 1, the hot-dip galvanizing liquid with alloy added prepared in this comparative example was used to perform hot-dip galvanizing on the substrate to be plated.

[0125] The thickness of the batch hot-dip galvanized coating obtained in this comparative example was tested by a magnetic thickness gauge, and a salt spray corrosion resistance test was performed. After removing the corrosion products of the batch hot-dip galvanized coating, the average corrosion weight loss change within 15 neutral salt spray test cycles was statistically analyzed to obtain the average corrosion rate. The results are shown in Table 1.

[0126] Comparative Example 9:

[0127] This comparative example provides a hot-dip galvanizing solution with alloy addition and a preparation method thereof, which comprises

[0128] 1) melting Al raw material, Ni raw material, Zr raw material, Sc raw material, Bi raw material, Re raw material and Zn raw material with good proportion to prepare a multi-element alloy;

[0129] 2) placing the multi-component alloy prepared in step 1) in a stone square cage, immersing it in molten zinc liquid, and moving it back and forth in the zinc pot until the multi-component alloy is completely melted, so that the alloy element components are evenly dissolved in the zinc liquid, thereby preparing a hot-dip galvanizing liquid with added alloy;

[0130] The alloy-added hot-dip galvanizing solution contains the following alloy element components in mass percentage: Al: 0.03%; Ni: 0.008%; Zr: 0.00027%; Sc: 0.0008%; Bi: 0.010%; Re: 0.005%; the remainder is Zn and unavoidable impurities.

[0131] As described in Example 1, the hot-dip galvanizing liquid with alloy added prepared in this comparative example was used to perform hot-dip galvanizing on the substrate to be plated.

[0132] The thickness of the batch hot-dip galvanized coating obtained in this comparative example was tested by a magnetic thickness gauge, and a salt spray corrosion resistance test was performed. After removing the corrosion products of the batch hot-dip galvanized coating, the average corrosion weight loss change within 15 neutral salt spray test cycles was statistically analyzed to obtain the average corrosion rate. The results are shown in Table 1.

[0133] Comparative Example 10

[0134] This comparative example provides a hot-dip galvanizing solution with alloy addition and a preparation method thereof, which comprises

[0135] 1) melting Al raw material, Ni raw material, Zr raw material, Sc raw material, Pr raw material, Bi raw material, Re raw material and Zn raw material with good proportion to prepare a multi-element alloy;

[0136] 2) placing the multi-component alloy prepared in step 1) in a stone square cage, immersing it in molten zinc liquid, and moving it back and forth in the zinc pot until the multi-component alloy is completely melted, so that the alloy element components are evenly dissolved in the zinc liquid, thereby preparing a hot-dip galvanizing liquid with added alloy;

[0137] The alloy-added hot-dip galvanizing solution contains the following alloy element components in mass percentage: Al: 0.03%; Ni: 0.008%; Zr: 0.00027%; Sc: 0.0008%; Pr: 0.005%; Bi: 0.010%; Re: 0.005%; the remainder is Zn and unavoidable impurities.

[0138] As described in Example 1, the hot-dip galvanizing liquid with alloy added prepared in this comparative example was used to perform hot-dip galvanizing on the substrate to be plated.

[0139] The thickness of the batch hot-dip galvanized coating obtained in this embodiment was tested by a magnetic thickness gauge, and a salt spray corrosion resistance test was performed. After removing the corrosion products of the batch hot-dip galvanized coating, the average corrosion weight loss change within 15 neutral salt spray test cycles was statistically analyzed to obtain the average corrosion rate. The results are shown in Table 1.

[0140] Table 1

[0141]

[0142] From the comparison of the results of Examples 1-5 and Comparative Examples 1-4, it can be seen that the addition of Zr or Sc can reduce the thickness of the coating, but the effect of adding both at the same time is more significant and has a synergistic effect.

[0143] From the comparison of the results of Examples 1-5 and Comparative Examples 5-6, it can be seen that when the ratio of Sc to Zr is 3 / 1, the effect of thinning and increasing corrosion resistance is most significant.

[0144] From the comparison of the results of Examples 1-5 and Comparative Examples 7-8, it can be seen that when the contents of Sc and Zr are higher than the range defined in the present invention, the effects of thinning and increasing corrosion resistance begin to decline.

[0145] From the comparison of the results of Examples 1-5 and Comparative Examples 9-10, it can be seen that when Pr is added, the coating thickness can be significantly reduced and the corrosion resistance can be increased, while when Pr is added in excess, the effect of thinning and increasing corrosion resistance decreases.

[0146] In the description of the specification, the description with reference to the terms "one embodiment", "specific embodiment", "example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more implementations or examples in a suitable manner.

Claims

1. A hot-dip galvanizing solution with alloy addition, comprising the following alloy element components in mass percentage: Al: 0.025-0.030%; Ni: 0.005%-0.009%; Zr: 0.0002-0.0003%; Sc: 0.0006-0.0009%; Pr:0.002-0.003%; Bi: 0.004-0010%; Re: 0.001-0.005%; the balance is Zn and unavoidable impurities, wherein the ratio of Sc / Zr is 3 / 1.

2. The alloy-added hot-dip galvanizing solution of claim 1, comprising the following alloy element components in mass percentage: Al: 0.025-0.030%; Ni: 0.005%-0.009%; Zr: 0.0002%; Sc: 0.0006%; Pr:0.002-0.003%; Bi: 0.004-0010%; Re: 0.001-0.005%; the balance is Zn and inevitable impurities.

3. The alloy-added hot-dip galvanizing solution of claim 1, comprising the following alloy element components in mass percentage: Al: 0.025-0.030%; Ni: 0.005%-0.009%; Zr: 0.0003%; Sc: 0.0009%; Pr:0.002-0.003%; Bi: 0.004-0010%; Re: 0.001-0.005%; the balance is Zn and inevitable impurities.

4. A method for preparing the alloy-added hot-dip galvanizing solution according to any one of claims 1 to 3, comprising 1) melting Al raw material, Ni raw material, Zr raw material, Sc raw material, Pr raw material, Bi raw material, Re raw material and Zn raw material with good proportion to prepare a multi-element alloy; 2) The multi-component alloy of step 1) is placed in a stone square cage, immersed in molten zinc liquid, and moved back and forth in the zinc pot until the multi-component alloy is completely melted, so that the alloy element components are evenly dissolved in the zinc liquid to prepare a hot-dip galvanizing liquid with added alloy.