Production method of thin-gauge weathering steel for photovoltaic support

In the production of thin-spec weathering steel for photovoltaic brackets, the use of CSiMn component system and corrosion-resistant elements are used to simplify the metallurgical sheet production process, solve the problems of high cost and complex production of existing weathering steel, and achieve low cost and high strength Weather resistant steel production meets industrial needs.

CN118932255AActive Publication Date: 2024-11-12BAOTOU IRON & STEEL (GROUP) CO LTD

Patent Information

Application Number
CN202410943922.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-12
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

The existing weathering steel is costly in photovoltaic bracket applications, and the metallurgical sheet production process is complex, making it difficult to meet the needs of industrial production.

Method used

The CSiMn component system is used to add corrosion-resistant elements Cu, P, Cr, and through the smelting-continuous casting and hot rolling production process, the alloy element content is reduced, the production process is simplified, and the atmospheric corrosion resistance of steel is improved.

Benefits of technology

It has achieved low-cost production of high-strength photovoltaic brackets with thin specifications, and its mechanical properties and process performance meet relevant standards, which are suitable for industrial production and reduce production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932255A_ABST
    Figure CN118932255A_ABST
Patent Text Reader

Abstract

The invention discloses a production method of thin-gauge weathering resistant steel for a photovoltaic support. The production method comprises a smelting-continuous casting production technological process. A hot rolling production technological process; the casting blank tapping temperature is 1240 + / -20 DEG C, the finish rolling temperature of finish rolling is 890 + / -10 DEG C, the cooling speed is 10-20 DEG C / S, and the thickness of a hot rolled steel strip is 1.8-2.5 mm; laminar cooling is adopted, and the coiling temperature is 650 + / -10 DEG C; the weathering resistant steel comprises the following chemical components in percentage by mass: 0.06 to 0.08 percent of C, 0.15 to 0.25 percent of S i, 0.35 to 0.45 percent of Mn, 0.03 to 0.04 percent of P, less than or equal to 0.001 percent of S, 0.26 to 0.30 percent of Cu, 0.55 to 0.65 percent of Cr, 0.020 to 0.030 percent of Ti and the balance of iron and impurities. A conventional C, S, i and Mn component system design is adopted, the element content of the corrosion-resistant alloy is properly reduced, and the production cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgical plate production, and in particular relates to a production method of thin-gauge weathering steel for photovoltaic brackets. Background Art

[0002] Atmospheric corrosion resistant steel (weathering steel) refers to a low alloy steel with good atmospheric corrosion resistance, which is made by adding a certain amount of Cu, P, C or Ni, Mo, Nb, Ti and other alloy elements to the steel. In industrial and rural atmospheric environments, weathering steel has excellent atmospheric corrosion resistance and other properties because it forms a dense and stable oxide protective film on the surface of its substrate, which hinders the entry of corrosive media. However, the rust layer formed by corrosion on the surface of ordinary carbon steel substrate has a loose structure and micro-cracks, which cannot really protect the substrate steel. Summary of the invention

[0004] The purpose of the present invention is to provide a production method of thin-gauge weathering steel for photovoltaic brackets. The conventional CSiMn component system is designed, and the corrosion-resistant elements Cu, P, and Cr are added to appropriately reduce the content of corrosion-resistant alloy elements and reduce production costs. The product is mainly used in the production of painting-free photovoltaic brackets.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0006] The present invention provides a method for producing thin-gauge weathering steel for photovoltaic brackets, comprising:

[0007] Smelting-continuous casting production process: molten iron pretreatment-converter-LF refining-casting machine;

[0008] Hot rolling production process: slab heating - high-pressure water descaling - fixed width press - E1R1 roughing mill rolling - E2R2 roughing mill rolling - flying shear - high-pressure water descaling - F1-F7 finishing mill rolling - encrypted laminar cooling - coiling - storage - sampling, inspection - weighing, packaging;

[0009] in:

[0010] The temperature of the billet out of the furnace is 1240±20℃, the final rolling temperature of the finishing rolling is 890±10℃, the cooling rate is 10-20℃ / S, and the thickness of the hot-rolled steel strip is 1.8-2.5mm; the cooling adopts laminar cooling equipment, front dispersion cooling mode, and the coiling temperature is 650±10℃;

[0011] The mass percentage of the chemical composition of the thin-gauge weathering steel for the photovoltaic support is: C: 0.06-0.08%, Si: 0.15-0.25%, Mn: 0.35-0.45%, P: 0.03-0.04%, S: ≤0.001%, Cu: 0.26-0.30%, Cr: 0.55-0.65%, Ti: 0.020-0.030%, and the rest is Fe and unavoidable impurities.

[0012] Furthermore, the mass percentage of the chemical composition of the thin-gauge weathering steel for the photovoltaic support is: C: 0.07%, Si: 0.20%, Mn: 0.38%, P: 0.035%, S: 0.004%, Cu: 0.28%, Cr: 0.56%, Ti: 0.021%, and the rest is Fe and unavoidable impurities.

[0013] Furthermore, the mass percentage of the chemical composition of the thin-gauge weathering steel for the photovoltaic support is: C: 0.07%, Si: 0.22%, Mn: 0.38%, P: 0.036%, S: 0.004%, Cu: 0.28%, Cr: 0.58%, Ti: 0.019%, and the rest is Fe and unavoidable impurities.

[0014] Furthermore, the mass percentage of the chemical composition of the thin-gauge weathering steel for the photovoltaic support is: C: 0.07%, Si: 0.20%, Mn: 0.39%, P: 0.033%, S: 0.003%, Cu: 0.28%, Cr: 0.59%, Ti: 0.019%, and the rest is Fe and unavoidable impurities.

[0015] Furthermore, the molten iron is pretreated with desulfurization, and top and bottom combined blowing converter is used to dephosphorize and decarbonize the molten iron to obtain molten steel. Argon is blown throughout the converter smelting process, scrap steel is added to the converter, and the converter tapping temperature is 1620°C; the molten steel after converter smelting is then subjected to LF off-furnace refining, the refining temperature is ≥1560°C, and the LF off-furnace refining is performed for temperature measurement and composition fine-tuning; the slab continuous casting overheat is 25°C, followed by slab cleaning, slow cooling, and continuous casting slab quality inspection; the slab heating temperature is 1230°C, the heating time is 43min, and a hot rolling mill is used for rolling; the finishing rolling temperature is 890°C, and the finished product thickness is 2mm; laminar cooling adopts front dispersion cooling, the cooling rate is 14°C / S, and the steel strip temperature is reduced to 646°C for coiling; finally, the product performance is tested.

[0016] Furthermore, the molten iron is pretreated with desulfurization, and top and bottom combined blowing converter is used to dephosphorize and decarbonize the molten iron to obtain molten steel. Argon is blown throughout the converter smelting process, scrap steel is added to the converter, and the converter tapping temperature is 1623°C; the molten steel after converter smelting is then subjected to LF off-furnace refining, the refining temperature is ≥1560°C, and the LF off-furnace refining is performed for temperature measurement and composition fine-tuning; the slab continuous casting overheat is 25°C, followed by slab cleaning, slow cooling, and continuous casting slab quality inspection; the slab heating temperature is 1235°C, the heating time is 45min, and a hot rolling mill is used for rolling; the finishing rolling temperature is 893°C, and the finished product thickness is 2mm; laminar cooling adopts front dispersion cooling, the cooling rate is 14°C / S, and the steel strip temperature is reduced to 650°C for coiling; finally, the product performance is tested.

[0017] Furthermore, the molten iron is pretreated with desulfurization, and top and bottom combined blowing converter is used to dephosphorize and decarbonize the molten iron to obtain molten steel. Argon is blown throughout the converter smelting process, scrap steel is added to the converter, and the converter tapping temperature is 1633°C; the molten steel after converter smelting is then subjected to LF off-furnace refining, the refining in-situ temperature is ≥1560°C, and the LF off-furnace refining is performed for temperature measurement and composition fine-tuning; the slab continuous casting overheat is 20°C, followed by slab cleaning, slow cooling, and continuous casting slab quality inspection; the slab heating temperature is 1250°C, the heating time is 49min, and the hot rolling mill is used for rolling; the finishing rolling temperature is 899°C, and the finished product thickness is 2mm; laminar cooling adopts front dispersion cooling, the cooling rate is 14°C / S, and the steel strip temperature is reduced to 653°C for coiling; finally, the product performance is tested.

[0018] Compared with the prior art, the beneficial technical effects of the present invention are:

[0019] The metallographic microstructure of the present invention is mainly ferrite, containing a small amount of pearlite. The grain size is between 11 and 11.5. The 500MPa hot-rolled high-strength structural steel produced by the method provided by the present invention has been tested for use in automobile factories, and the surface quality and performance indicators have met the relevant technical standards of automobile factories and the use requirements of relevant automobile factories. The mechanical properties and process properties meet the relevant standards and user requirements. At the same time, the alloy of the present invention has low cost, simple preparation method, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The present invention will be further described below in conjunction with the accompanying drawings.

[0021] Figure 1 This is the microstructure diagram of Example 1 of the present invention. DETAILED DESCRIPTION

[0022] The present invention is described in more detail below through specific examples. The examples are only descriptions of the best mode of implementation of the present invention and do not limit the scope of the present invention in any way.

[0023] Example 1

[0024] The molten iron is pre-treated for desulfurization, and the top and bottom combined blown converter is used to dephosphorize and decarbonize the molten iron to obtain molten steel. Argon is blown throughout the converter smelting process, and scrap steel is added to the converter. The converter tapping temperature is 1630℃. Then the molten steel after converter smelting is subjected to LF refining outside the furnace, and the refining temperature is ≥1560℃. The LF refining outside the furnace is used for temperature measurement and composition fine-tuning. The chemical composition of the LF refining casting machine is shown in Table 1. After the LF treatment, calcium treatment is carried out. After calcium treatment, the soft blowing time is guaranteed to be more than 8 minutes. . The overheat of the slab continuous casting is 25℃, and then the slab is cleaned, slowly cooled, and the quality of the continuous casting is checked. The slab heating temperature is 1230℃, the heating time is 205min, and the heated slab is dephosphorized by high-pressure water. The width is set by a fixed width press, and 2-stand rough rolling and 7-stand CVC finishing rolling are used. The finishing rolling temperature is 890℃, and the finished product thickness is 7mm. Laminar cooling adopts front dispersion cooling, the temperature of the steel strip is reduced to 590℃ for coiling, and finally the product performance is tested.

[0025] Example 2

[0026] The molten iron is pre-treated for desulfurization, and the top and bottom combined blown converter is used to decarbonize and dephosphorize the molten iron to obtain molten steel. Argon is blown throughout the converter smelting process, and scrap steel is added to the converter. The converter tapping temperature is 1630℃. Then the molten steel after converter smelting is subjected to LF refining outside the furnace, and the refining temperature is ≥1560℃. The LF refining outside the furnace is subjected to temperature measurement and composition fine-tuning. The chemical composition of the LF refining casting machine is shown in Table 1. After the LF treatment, calcium treatment is carried out. After calcium treatment, the soft blowing time is ensured to be more than 8 minutes. The overheat of the slab continuous casting is 30℃, and then the slab is cleaned, slowly cooled, and the quality of the continuous casting is checked. The slab heating temperature is 1235℃, and the heating time is 210min. The heated slab is dephosphorized by high-pressure water. The width is set by a fixed width press, and 2-stand rough rolling and 7-stand CVC finishing rolling are used. The finishing rolling temperature is 896℃, and the finished product thickness is 7mm. Laminar cooling adopts front dispersion cooling, the temperature of the steel strip is reduced to 582℃ for coiling, and finally the product performance is tested.

[0027] Example 3

[0028] The molten iron is pre-treated for desulfurization, and the top and bottom combined blown converter is used to decarbonize and dephosphorize the molten iron to obtain molten steel. Argon is blown throughout the converter smelting process, and scrap steel is added to the converter. The converter tapping temperature is 1628℃. Then the molten steel after converter smelting is subjected to LF refining outside the furnace, and the refining temperature is ≥1560℃. The LF refining outside the furnace is subjected to temperature measurement and composition fine-tuning. The chemical composition of the LF refining casting machine is shown in Table 1. After the F treatment, calcium treatment is carried out. After calcium treatment, the soft blowing time is ensured to be more than 8 minutes. The overheat of the slab continuous casting is 28℃, and then the slab is cleaned, slowly cooled, and the quality of the continuous casting is checked. The slab heating temperature is 1233℃, the heating time is 205min, and the heated slab is dephosphorized by high-pressure water. The width is set by a fixed width press, and 2-stand rough rolling and 7-stand CVC finishing rolling are used. The final rolling temperature of the finishing rolling is 896℃, and the thickness of the finished product is 7mm. Laminar cooling adopts front dispersion cooling, the temperature of the steel strip is reduced to 593℃ for coiling, and finally the product performance is tested.

[0029] Table 1 Chemical composition of Examples 1-3 of the present invention (wt%)

[0030] Example C Si Mn P S Alt Nb Ti 1 0.07 0.10 0.77 0.016 0.003 0.029 0.032 0.036 2 0.07 0.12 0.75 0.018 0.004 0.027 0.030 0.036 3 0.07 0.10 0.77 0.015 0.003 0.035 0.033 0.036

[0031] The steel coils of Examples 1 to 3 of the present invention were tested for mechanical properties, and the test results are shown in Table 2.

[0032] Table 2 Mechanical properties of the steel coils of Examples 1-3 of the present invention

[0033]

[0034]

[0035] It can be seen from the data in Table 2 that the mechanical properties and process properties of the 500MPa grade hot-rolled high-strength structural steel produced according to the method provided by the present invention meet the requirements of the agreement signed with the user.

[0036] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for producing thin-gauge weathering steel for photovoltaic brackets, characterized in that: include: Smelting-continuous casting production process: molten iron pretreatment-converter-LF refining-casting machine; Hot rolling production process: slab heating - high-pressure water descaling - fixed width press - E1R1 roughing mill rolling - E2R2 roughing mill rolling - flying shear - high-pressure water descaling - F1-F7 finishing mill rolling - encrypted laminar cooling - coiling - storage - sampling, inspection - weighing, packaging; in: The temperature of the billet out of the furnace is 1240±20℃, the final rolling temperature of the finishing rolling is 890±10℃, the cooling rate is 10-20℃ / S, and the thickness of the hot-rolled steel strip is 1.8-2.5mm; the cooling adopts laminar cooling equipment, front dispersion cooling mode, and the coiling temperature is 650±10℃; The mass percentage of the chemical composition of the thin-gauge weathering steel for the photovoltaic support is: C: 0.06-0.08%, Si: 0.15-0.25%, Mn: 0.35-0.45%, P: 0.03-0.04%, S: ≤0.001%, Cu: 0.26-0.30%, Cr: 0.55-0.65%, Ti: 0.020-0.030%, and the rest is Fe and unavoidable impurities.

2. The method for producing thin-gauge weathering steel for photovoltaic brackets according to claim 1, characterized in that: The mass percentage of the chemical composition of the thin-gauge weathering steel for the photovoltaic support is: C: 0.07%, Si: 0.20%, Mn: 0.38%, P: 0.035%, S: 0.004%, Cu: 0.28%, Cr: 0.56%, Ti: 0.021%, and the rest is Fe and unavoidable impurities.

3. The method for producing thin-gauge weathering steel for photovoltaic brackets according to claim 1, characterized in that: The mass percentage of the chemical composition of the thin-gauge weathering steel for the photovoltaic support is: C: 0.07%, Si: 0.22%, Mn: 0.38%, P: 0.036%, S: 0.004%, Cu: 0.28%, Cr: 0.58%, Ti: 0.019%, and the rest is Fe and unavoidable impurities.

4. The method for producing thin-gauge weathering steel for photovoltaic brackets according to claim 1, characterized in that: The mass percentage of the chemical composition of the thin-gauge weathering steel for the photovoltaic support is: C: 0.07%, Si: 0.20%, Mn: 0.39%, P: 0.033%, S: 0.003%, Cu: 0.28%, Cr: 0.59%, Ti: 0.019%, and the rest is Fe and unavoidable impurities.

5. The method for producing thin-gauge weathering steel for photovoltaic brackets according to claim 2, characterized in that: The molten iron is pre-treated with desulfurization, and top and bottom combined blowing converter is used to dephosphorize and decarbonize the molten iron to obtain molten steel. Argon is blown throughout the converter smelting process, scrap steel is added to the converter, and the converter tapping temperature is 1620℃; the molten steel after converter smelting is then subjected to LF refining outside the furnace, and the refining temperature is ≥1560℃, and the LF refining is performed for temperature measurement and composition fine-tuning; the overheat degree of slab continuous casting is 25℃, followed by slab cleaning, slow cooling, and continuous casting slab quality inspection; the slab heating temperature is 1230℃, the heating time is 43min, and hot rolling mill is used for rolling; the finishing rolling temperature is 890℃, and the finished product thickness is 2mm; laminar cooling adopts front dispersion cooling, the cooling rate is 14℃ / S, and the steel strip temperature is reduced to 646℃ for coiling; finally, product performance testing is carried out.

6. The method for producing thin-gauge weathering steel for photovoltaic brackets according to claim 3, characterized in that: The molten iron is pre-treated with desulfurization, and top and bottom combined blowing converter is used to dephosphorize and decarbonize the molten iron to obtain molten steel. Argon is blown throughout the converter smelting process, scrap steel is added to the converter, and the converter tapping temperature is 1623℃; the molten steel after converter smelting is then subjected to LF refining outside the furnace, and the refining temperature is ≥1560℃, and the LF refining is performed for temperature measurement and composition fine-tuning; the overheat degree of slab continuous casting is 25℃, followed by slab cleaning, slow cooling, and continuous casting slab quality inspection; the slab heating temperature is 1235℃, the heating time is 45min, and hot rolling mill is used for rolling; the finishing rolling temperature is 893℃, and the finished product thickness is 2mm; laminar cooling adopts front dispersion cooling, the cooling rate is 14℃ / S, and the steel strip temperature is reduced to 650℃ for coiling; finally, product performance testing is carried out.

7. The method for producing thin-gauge weathering steel for photovoltaic brackets according to claim 4, characterized in that: The molten iron is pre-treated for desulfurization, and the top and bottom combined blowing converter is used to dephosphorize and decarbonize the molten iron to obtain molten steel. Argon is blown throughout the converter smelting process, scrap steel is added to the converter, and the converter tapping temperature is 1633℃; the molten steel after converter smelting is then subjected to LF refining outside the furnace, and the refining temperature is ≥1560℃. The LF refining outside the furnace is performed for temperature measurement and composition fine-tuning; the slab continuous casting overheat is 20℃, and then the slab is cleaned, slowly cooled, and the continuous casting slab quality is checked; the slab heating temperature is 1250℃, the heating time is 49min, and the hot rolling mill is used for rolling; finishing rolling The final rolling temperature is 899℃, and the finished product thickness is 2mm; the laminar cooling adopts front dispersion cooling, and the cooling rate is 14℃ / S. The temperature of the steel strip is lowered to 653℃ for coiling; finally, the product performance is tested.

Citation Information

Patent Citations

  • Titanium-containing low-nickel high-strength weathering steel and production method thereof

    CN106591707A

  • Molten steel of chromium vanadium titanium containing atmospheric corrosion resistant steel as well as atmospheric corrosion resistant steel and production method thereof

    CN106676400A

  • Weather-resistant checkered steel plate and production method thereof

    CN108971225A

  • Method for improving impact toughness of weathering steel

    CN115927954A

  • Production method of high-weather-resistance coating-free steel for photovoltaic support

    CN116732419A

Cited By

  • Production method of 700MPa-grade high-strength weathering steel

    CN120041745A

  • Steel with yield strength of 500MPa for zinc-aluminum-magnesium-plated high-light photovoltaic bracket and preparation method of steel for zinc-aluminum-magnesium-plated high-light photovoltaic bracket