A kind of manufacturing process of cashmere core-spun yarn
By adding core yarn unwinding device on the yarn machine and using two rovings to feed, the problem of poor cashmere clad core yarn is solved, and the complete coating of core yarn and product quality is improved.
Patent Information
- Application Number
- CN202211526674.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-30
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-11-30
AI Technical Summary
In the existing core-covered yarn manufacturing process, the cashmere core-covered yarn has poor effect, resulting in the core-covered yarn being exposed and the product quality is not high.
Add a core yarn unwinding device on the yarn machine to ensure that the output of the core yarn is consistent with the feeding tension, and complete coverage of the core yarn is achieved by feeding 2 rovings.
Complete coverage of the core yarn is achieved, avoiding exposure of the core yarn and improving product quality.
Smart Images

Figure CN115852546B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of core-spun yarn manufacturing, in particular to a manufacturing process of cashmere core-spun yarn. Background Art
[0002] Core-spun yarn is a popular product in the domestic market and the European and American markets. In addition to its special structure, core-spun yarn has many advantages. It can make full use of the excellent physical properties of the core yarn, the performance and surface characteristics of the outer fiber, give full play to the advantages of the two fibers and make up for their shortcomings. For example, polyester-cotton core-spun yarn can give full play to the advantages of polyester filaments, such as being straight, anti-bending, easy to wash and dry, while at the same time giving full play to the advantages of the outer cotton fiber, such as good moisture absorption, less static electricity, and not easy to pilling. Core-spun yarn can also take advantage of the different chemical properties of chemical fiber filaments and outer fibers. During the dyeing and finishing of fabrics, chemicals are used to rot a part of the outer fiber to make a rotten fabric with a three-dimensional pattern effect, which is one of the effective ways to increase product added value and expand market space.
[0003] Cashmere is known as "soft gold". Cashmere contains a lot of air and forms an air layer, which can defend against the invasion of external cold air and has a good thermal insulation effect. The outer scales of cashmere are also finer and smoother than other fibers, and are light, soft, tender and smooth.
[0004] In recent years, core-spun yarns have become more and more popular, such as core-spun yarns with polyester cores covered by viscose, viscose and linen or cotton and viscose blends, core-spun yarns covered by cotton and silk or cotton and wool blends, etc. The preparation of traditional core-spun yarns is completed on spinning machines, but during the preparation process, the core yarn is difficult to be completely covered, and the core yarn is often exposed; because cashmere is soft and light, it is even more difficult to use cashmere to prepare core-spun yarns. Therefore, the existing manufacturing process of core-spun yarns needs to be further improved. Summary of the invention
[0005] The purpose of the present invention is to make up for the above-mentioned shortcomings and provide a manufacturing process for cashmere core-spun yarn with good covering effect and high product quality.
[0006] The technical solution of the present invention is achieved in this way:
[0007] A manufacturing process of cashmere core-spun yarn comprises the following steps:
[0008] Step 1: Welding: Weld the cashmere raw materials on a fully automatic welding machine, add welding oil and antistatic agent, and cure for 24 hours after welding;
[0009] Step 2: Combing: The cashmere raw materials that have been cured for 24 hours are combed with a combing machine to fully loosen and comb the fibers to make them parallel, straight and fully mixed, and the combed fibers are twisted into coarse yarns of set specifications;
[0010] Step 3, spinning: a spinning frame is used for spinning operation, wherein the spinning frame is provided with a core yarn roller and a roving roller, the yarn outlet of the core yarn roller is provided with a core yarn unwinding roller, and the yarn outlet of the roving roller is provided with a roving unwinding roller, the roving is blended with the roving through the roving unwinding roller, the core line sensor, the core line bundler, and the front roller; the roving is blended with the core yarn through the roving unwinding roller, the upper roller, the false twister, the back roller, the first middle roller, and the second middle roller; cashmere fiber is used as the outer roving and polyester is used as the core yarn. The core yarn passes through the core yarn unwinding roller, passes through the core line bundler, and merges with the cashmere fiber output from the front roller at an angle of 30°. By controlling the speed ratio between the core yarn and the drafting output cashmere yarn to be 1:1.15, the cashmere fiber is wrapped around the core yarn through ring twisting to spin into core-spun yarn;
[0011] Step 4: Winding: The yarn from the previous spinning process is wound by a winding machine, and the defects on the yarn are cleaned;
[0012] Step 5: doubling: use a doubling machine to doubling two strands of qualified yarn after winding, with a speed of 600m / min and a fixed length of 14300m;
[0013] Step 6: Double twisting: Use a double twisting machine to add a set twist to the two strands of yarn combined together, double yarn twist: 320T / M; twist direction: S twist; speed: 6500rpm.
[0014] The measures to further optimize this technical solution are:
[0015] As an improvement, in the step three, two rovings are fed into the upper roller at the same time.
[0016] As an improvement, according to the weight ratio of cashmere fiber and polyester core yarn, the ratio of cashmere fiber is 90%-95%, and the ratio of polyester core yarn is 5%-10%.
[0017] As an improvement, the crude oil is FX-906, and the addition ratio is 3.5% of the weight of the raw material; the antistatic agent is FX-AS301, and the addition ratio is 1% of the weight of the raw material.
[0018] As an improvement, in the step 1, the moisture regain of the wool is controlled at 24%±1%.
[0019] As an improvement, the gauge between section A of the combing machine and the working roller is 0.5-0.6mm, and the gauge between section A and the doffer is 0.45mm; the gauge between section B and the working roller is 0.35-0.5mm, and the gauge between section B and the doffer is 0.3mm; the gauge between section C and the working roller is 0.3-0.4mm, and the gauge between section C and the doffer is 0.25mm; the gauge between section D and the working roller is 0.25-0.3mm, and the gauge between section D and the doffer is 0.2mm.
[0020] As an improvement, the speed ratio of section A of the combing machine to the working roller is 188 / 2.5; the speed ratio of section B to the working roller is 360 / 2.5, and the speed ratio of section B to the doffer is 360 / 17; the speed ratio of section C to the working roller is 360 / 2.5, and the speed ratio of section C to the doffer is 360 / 21; the speed ratio of section D to the working roller is 360 / 2.5, and the speed ratio of section D to the doffer is 390 / 21.
[0021] As an improvement, on the combing machine, the combing roving fixed weight is: 0.77g / 15m, the sliver output speed is: 20m / min, the wool feeding amount is: 330g, and the wool feeding cycle is: 70s.
[0022] As an improvement, the spinning count on the ring spinning frame is set as follows: 2 / 26Nm, the yarn draft is controlled at 1.2-1.4; the twist is 580T / M; the twist direction is Z twist; and the spindle speed is 2500-4500rpm.
[0023] The advantages of the present invention compared with the prior art are:
[0024] When spinning the core-spun yarn, the present invention improves the structure of the spinning frame on the basis of a traditional spinning frame, adds a core yarn unwinding device, so that the output of the core yarn is consistent with the feeding tension, achieves complete covering of the core yarn, avoids exposure of the core yarn, and improves product quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a schematic structural diagram of the spinning frame of the present invention.
[0026] In the figure: core yarn roller 1, core yarn unwinding roller 11, roving roller 2, roving unwinding roller 21, core wire sensor 3, core wire buncher 4, front roller 5, upper roller 6, false twister 7, rear roller 8, first middle roller 91, second middle roller 92. DETAILED DESCRIPTION
[0027] The present invention provides a manufacturing process of cashmere core-spun yarn, comprising the following steps:
[0028] Step 1: Mixing: Mix the cashmere raw materials on a fully automatic mixing machine, add mixing oil and antistatic agent, and cure for 24 hours after mixing.
[0029] Step 2: Combing: The cashmere raw materials that have been cured for 24 hours are combed with a combing machine to fully loosen and comb the fibers to make them parallel, straight and fully mixed. The combed fibers are rubbed into coarse yarn of set specifications through belt wires, split shafts and leather boards.
[0030] Step 3, spinning: a spinning frame is used for spinning operation, wherein the spinning frame is provided with a core yarn roller 1 and a roving roller 2, the yarn outlet of the core yarn roller 1 is provided with a core yarn unwinding roller 11, the yarn outlet of the roving roller 2 is provided with a roving unwinding roller 21, the roving is blended with the roving through the roving unwinding roller 21, the core line sensor 3, the core line bundler 4, and the front roller 5; the roving is blended with the roving through the roving unwinding roller 21, the upper roller 6, and the false twister 7 , the back roller 8, the first middle roller 91, the second middle roller 92 and the core yarn are blended; cashmere fiber is used as the outer roving, polyester is used as the core yarn, the core yarn is passed through the core yarn unwinding roller 21, through the core yarn bundler 4, and merged with the cashmere fiber output from the front roller mouth at an angle of 30°, by controlling the speed ratio between the core yarn and the drafting output cashmere yarn to 1:1.15, through ring twisting, the cashmere fiber wraps around the core yarn and spins into core-spun yarn. As a further improvement, two rovings are fed to the upper roller 6 at the same time.
[0031] The function of the spinning frame is to evenly draw the qualified roving to the required linear density, add appropriate twist to the drafted sliver, give the yarn certain physical and mechanical properties such as strength, elasticity and gloss, and finally wind the spun yarn into shape according to certain requirements for easy transportation, storage and subsequent processing. In order to ensure the tension of the core yarn, a set of core yarn unwinding device is added to the traditional ring spinning frame so that the output of the core yarn is always consistent with the feeding tension. In addition, two rovings are fed to achieve perfect coating and improve quality.
[0032] Step 4, winding: The yarn from the previous spinning process is wound by a winding machine, and the defects such as thick sections, thin sections, double yarns, weak twisted yarns, cotton knots, impurities, etc. on the yarn are cleaned. It is worth noting that the core wire cannot be missing at the joint.
[0033] Step 5: Parallel yarn: Parallel yarn is processed by paralleling machine, the speed is 600m / min, and the fixed length is 14300m. It is worth noting that the core wire should not be missing at the joint, and the two yarns should be pulled evenly to avoid braided yarn.
[0034] Step 6, double twisting: Use a double twisting machine to add a set twist to the two strands of yarn combined, double yarn twist: 320T / M; twist direction: S twist; speed: 6500rpm. Add a certain twist to the yarn to increase the strength of the yarn, improve the uniformity of the yarn, make the yarn more elastic, more wear-resistant, and have a better gloss and feel.
[0035] When choosing the core yarn, you can choose monofilaments and multifilaments of chemical fiber filaments, or single yarns spun from staple fibers. The fineness of the monofilaments and the number of monofilaments in the multifilaments should be selected according to the spinning count and the purpose of the fabric. If you choose a finer core yarn, the outer fiber layer can be thinner, the coating effect is better, and the final yarn count is high; conversely, if you choose a thicker core yarn, the outer fiber layer needs to be thicker, and the yarn count is low. For the core yarn of the same fineness, the finer the monofilament, the more roots, and the softer and smoother the fabric. Conversely, the fewer roots, the better the rigidity and stiffness of the fabric. It should be pointed out that when single yarns spun from staple fibers are used as core yarns, reverse twisting is required during the spinning process, and the twist of the core yarn is reduced. The yarn finally spun has a good feel, good fluffiness, and good air permeability, which is suitable for making spring and summer knitted fabrics and clothing.
[0036] like Figure 1 As shown, the roving frame is provided with a core yarn roller 1 and a roving roller 2, the yarn outlet of the core yarn roller 1 is provided with a core yarn unwinding roller 11, and the yarn outlet of the roving roller 2 is provided with a roving unwinding roller 21. The core yarn is blended with the roving through the roving unwinding roller 21, the core wire sensor 3, the core wire buncher 4 and the front roller 5; the roving is blended with the core yarn through the roving unwinding roller 21, the upper roller 6, the false twister 7, the rear roller 8, the first middle roller 91 and the second middle roller 92.
[0037] According to the weight ratio of cashmere fiber and polyester core yarn, the ratio of cashmere fiber is 90%-95%, and the ratio of polyester core yarn is 5%-10%. In this embodiment, the ratio of cashmere fiber to polyester core yarn is 93%:7%.
[0038] The crude oil is FX-906, and the addition ratio is 3.5% of the weight of the raw material; the antistatic agent is FX-AS301, and the addition ratio is 1% of the weight of the raw material.
[0039] In the step 1, the moisture regain of the wool is controlled at 24%±1%.
[0040] On the combing machine, the gauge between section A of the cylinder and the working roller is 0.5-0.6mm, and the gauge between section A of the cylinder and the doffer is 0.45mm; the gauge between section B of the cylinder and the working roller is 0.35-0.5mm, and the gauge between section B of the cylinder and the doffer is 0.3mm; the gauge between section C of the cylinder and the working roller is 0.3-0.4mm, and the gauge between section C of the cylinder and the doffer is 0.25mm; the gauge between section D of the cylinder and the working roller is 0.25-0.3mm, and the gauge between section D of the cylinder and the doffer is 0.2mm.
[0041] The speed ratio of section A cylinder to the working roller on the combing machine is 188 / 2.5; the speed ratio of section B cylinder to the working roller is 360 / 2.5, and the speed ratio of section B cylinder to the doffer is 360 / 17; the speed ratio of section C cylinder to the working roller is 360 / 2.5, and the speed ratio of section C cylinder to the doffer is 360 / 21; the speed ratio of section D cylinder to the working roller is 360 / 2.5, and the speed ratio of section D cylinder to the doffer is 390 / 21.
[0042] On the wool combing machine, the wool roving fixed weight is 0.77 g / 15 m, the sliver output speed is 20 m / min, the wool feeding amount is 330 g, and the wool feeding cycle is 70 s.
[0043] On the ring spinning frame, the spinning count is set to: 2 / 26Nm, the yarn draft is controlled at 1.2-1.4; the twist is set to 580T / M; the twist direction is set to Z twist; and the spindle speed is set to 2500-4500rpm.
[0044] In the winding step, a winding machine is used for processing. Winding: tension voltage 6V, 3V, 0V; yarn clearer parameters are as follows:
[0045]
[0046] In the spinning of fine yarn, the tension of the core yarn has a great influence on the covering effect of the core yarn. When the tension of the core yarn is large, the output speed of the core yarn on the front roller 5 is too slow, while the output speed of the outer fiber (roving) is certain, which increases the entanglement of the outer fiber on the core yarn and causes the core yarn to have thick sections. If the tension of the core yarn is too large and exceeds the breaking tension of the core yarn, the core yarn is easy to break; when the core yarn breaks, the outer fiber continues to spin, resulting in the failure of the core yarn to be covered, thus forming a longer or shorter segment of pure velvet yarn, which also leads to a decrease in product quality. Therefore, the tension of the core yarn cannot be too large. When the tension of the core yarn is small, the output speed of the core yarn on the front roller 5 is too fast, and it cannot form the required speed difference with the output speed of the outer fiber (roving), so that the outer fiber is insufficiently covered on the core yarn, resulting in the phenomenon of core exposure. Excessive or too small tension of the core yarn will affect the covering effect. Therefore, in order to spin an ideal core yarn, the tension of the core yarn needs to be strictly controlled. In the present invention, a core yarn unwinding device is added through structural modification of the spinning frame, so that the output of the core yarn is consistent with the feeding tension; in addition, two coarse yarns are fed to achieve complete covering of the core yarn, avoid exposure of the core yarn, and improve product quality.
[0047] The best embodiment of the present invention has been described, and various changes or modifications may be made by those skilled in the art without departing from the scope of the present invention.
Claims
1. A manufacturing process of cashmere core-spun yarn, characterized by: The following steps are involved: Step 1, wool blending: woolen the cashmere raw materials on a fully automatic wool blending machine, add wool blending oil and antistatic agent, and cure the wool for 24 hours after blending; the wool blending oil is FX-906, and the addition ratio is 3.5% of the weight of the raw material; the antistatic agent is FX-AS301, and the addition ratio is 1% of the weight of the raw material. The moisture regain of the wool is controlled at 24%±1%; Step 2, combing: the cashmere raw material after 24 hours of health care is combed by a combing machine, the fibers are fully loosened and combed to make them parallel, straight and fully mixed, and the combed fibers are twisted into coarse yarns of set specifications; the spacing between the cylinder section A and the working roller on the combing machine is 0.5-0.6mm, and the spacing between the cylinder section A and the doffer is 0.45mm; the spacing between the cylinder section B and the working roller is 0.35-0.5mm, and the spacing between the cylinder section B and the doffer is 0.3mm; the spacing between the cylinder section C and the working roller is 0.3-0.4mm, and the spacing between the cylinder section C and the doffer is 0.25mm; the spacing between the cylinder section D and the working roller is 0.25-0 .3mm, the spacing between the cylinder section D and the doffer is 0.2mm; the speed ratio of the cylinder section A to the working roller on the combing machine is 188 / 2.5; the speed ratio of the cylinder section B to the working roller is 360 / 2.5, and the speed ratio of the cylinder section B to the doffer is 360 / 17; the speed ratio of the cylinder section C to the working roller is 360 / 2.5, and the speed ratio of the cylinder section C to the doffer is 360 / 21; the speed ratio of the cylinder section D to the working roller is 360 / 2.5, and the speed ratio of the cylinder section D to the doffer is 390 / 21; on the combing machine, the fixed weight of the combing roving is: 0.77g / 15m, the sliver output speed is: 20m / min, the wool feeding amount is: 330g, and the wool feeding cycle is: 70s; Step 3, spinning: a spinning frame is used for spinning operation, wherein the spinning frame is provided with a core yarn roller (1) and a roving roller (2), the yarn outlet of the core yarn roller (1) is provided with a core yarn unwinding roller (11), and the yarn outlet of the roving roller (2) is provided with a roving unwinding roller (21), the roving is blended with the roving through the roving unwinding roller (21), the core line sensor (3), the core line bundler (4), and the front roller (5); the roving is blended with the roving through the roving unwinding roller (21), the upper roller (6), the false twister (7), The back roller (8), the first middle roller (91), the second middle roller (92) and the core yarn are blended; cashmere fiber is used as the outer roving, polyester is used as the core yarn, the core yarn is passed through the core yarn unwinding roller (11), and through the core yarn bundler (4), it merges with the cashmere fiber output from the front roller mouth at an angle of 30 degrees, and the speed ratio between the core yarn and the drafting output cashmere yarn is controlled to be 1:1.15, and the cashmere fiber is twisted by the ring spindle to achieve the wrapping of the core yarn and the core-spun yarn; on the spinning machine, the spinning count is set to: 2 / 26 Nm, the yarn draft is controlled to be 1.2-1.4; the twist is: 580T / M; Twist direction: Z twist; spindle speed: 2500~4500 rpm; Step 4: Winding: The yarn from the previous spinning process is wound by a winding machine, and the defects on the yarn are cleaned; Step 5: doubling: use a doubling machine to doubling two strands of qualified yarn after winding, with a speed of 600m / min and a fixed length of 14300m; Step 6: Double twisting: Use a double twisting machine to add a set twist to the two strands of yarn, double yarn twist: 320T / M; Twist direction: S twist; Speed: 6500 rpm.
2. The manufacturing process of a cashmere core-spun yarn according to claim 1, characterized in that: In the step 3, two rovings are fed into the upper roller (6) at the same time.
3. The manufacturing process of a cashmere core-spun yarn according to claim 1, characterized in that: According to the weight ratio of cashmere fiber and polyester core yarn, the ratio of cashmere fiber is 90%-95%, and the ratio of polyester core yarn is 5%-10%.
Citation Information
Patent Citations
BE685404A
Segment color cashmere and yak wool core-spun yarn and production method thereof
CN105019086A
Cited By
Preparation process of wool spinning core-spun composite yarn
CN120250212A