A preparation method of lithium iron phosphate positive electrode material, positive electrode sheet and lithium ion battery

By regulating the mixing ratio and particle size of lithium iron phosphate materials, the problem of low compaction density of lithium iron phosphate materials is solved, the preparation of high compaction density cathode materials is achieved, the energy density and cycle performance of the battery are improved, and the battery is simplified. Process flow.

CN115863630BActive Publication Date: 2024-10-11SHENZHEN BYD LITHIUM BATTERY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111132574.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-26
Publication Date
2024-10-11
Estimated Expiration
2041-09-26

AI Technical Summary

Technical Problem

The compacted density of lithium iron phosphate materials is low, resulting in a low energy density of the battery. It is difficult to effectively improve the current method without increasing the risk of magnetic Fe exceeding the standard or complicating the process, and the blending ratio relationship is not clear.

Method used

By regulating the combination of two lithium iron phosphate materials and using different mass ratios to achieve the preparation of lithium iron phosphate cathode materials with high compaction density, the correlation between the blending ratio and compaction density was established, providing a fitting value to achieve controllable preparation of high compaction density.

Benefits of technology

It improves the filling rate and electrochemical performance of the cathode material to ensure excellent energy density and cycle performance of the battery, while simplifying the process and saving materials and time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115863630B_ABST
    Figure CN115863630B_ABST
Patent Text Reader

Abstract

The present application provides a method for preparing a lithium iron phosphate positive electrode material, comprising: mixing a first lithium iron phosphate material with a maximum compaction density A and a second lithium iron phosphate material with a maximum compaction density B according to a mass ratio of a:b to obtain a lithium iron phosphate positive electrode material; wherein a=0.315A-0.086B-0.25, b=1-a; C=0.61+0.37A+0.546B; C represents a fitted value of the maximum compaction density of the lithium iron phosphate positive electrode material, and the units of A, B, and C are all g / cm 3 , B greater than 2.5g / cm 3 , A at 1.7-2.5 g / cm 3 The preparation method can mix lithium iron phosphate materials with different compaction densities in a suitable proportion to prepare a lithium iron phosphate positive electrode material with a higher compaction density. The present application also provides a positive electrode sheet and a battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of lithium-ion batteries, and in particular to a method for preparing a lithium iron phosphate positive electrode material, a positive electrode sheet and a lithium-ion battery. Background Art

[0002] Lithium iron phosphate materials are widely used in power batteries due to their advantages such as high structural stability, good safety performance, moderate operating voltage and low cost. However, lithium iron phosphate has an obvious disadvantage: its compaction density is low and it is difficult to exceed 2.6g / cm 3 , which results in low energy density of batteries made from it and hinders the application of this material.

[0003] The existing methods for improving the compaction density of lithium iron phosphate materials are mainly divided into two categories: one is to simply increase the sintering temperature, but this method has limited improvement on the compaction density, and too high a sintering temperature will increase the risk of excessive magnetic Fe, greatly increasing the potential safety hazards of the battery. The second is to achieve different particle combinations by blending finished lithium iron phosphate products, thereby improving the compaction density, but the existing methods of this type do not give a clear relationship between the blending ratio, material characteristics, etc. of each lithium iron phosphate product and the required high compaction density of the positive electrode material after blending. Therefore, it is necessary to provide a controllable preparation method for battery positive electrode materials with high compaction density. Summary of the invention

[0004] In view of this, the present application provides a method for preparing a lithium iron phosphate positive electrode material, which realizes controllable adjustment of the high compaction density of the lithium iron phosphate positive electrode material mixed by regulating the combination of two lithium iron phosphate materials.

[0005] Specifically, in a first aspect, the present application provides a method for preparing a lithium iron phosphate positive electrode material, comprising the following steps:

[0006] The first lithium iron phosphate material with a maximum compaction density of A and the second lithium iron phosphate material with a maximum compaction density of B are mixed at a mass ratio of a:b to obtain a lithium iron phosphate positive electrode material;

[0007] Wherein, a=0.315A-0.086B-0.25, b=1-a;

[0008] C = 0.61 + 0.37A + 0.546B;

[0009] C represents the fitted value of the maximum compaction density of the lithium iron phosphate positive electrode material, and the units of A, B, and C are all g / cm 3 , the B is greater than 2.5g / cm 3 , the A is between 1.7 and 2.5 g / cm 3 within the range.

[0010] The preparation method of the positive electrode material provided in the embodiment of the present application is to mix two lithium iron phosphate materials with different maximum compaction densities and use them as positive electrode materials, and establish a certain relationship between the blending ratio a and b of the two and their maximum compaction density, so as to improve the filling rate and compaction density of the positive electrode material formed by the two, and then ensure that the electrochemical properties such as gram capacity and energy density of the battery made by the positive electrode material are also excellent. In addition, based on the maximum compaction density of the two lithium iron phosphate materials, a fitting value C of the maximum compaction density of the positive electrode material mixed by the two is given, and the fitting value is very close to the measured value, so the controllable preparation of the positive electrode material with the required high compaction density can be achieved based on the above relationship, without having to test the compaction density of the positive electrode sheet made of the obtained positive electrode material every time, saving materials and time.

[0011] In the embodiment of the present application, the C is greater than 2.6 g / cm 3 At this time, the compaction density of the positive electrode material is greater than that of the existing lithium iron phosphate positive electrode material. The a is less than 0.3225.

[0012] In the present application, the maximum compaction density B of the second lithium iron phosphate material is greater than the maximum compaction density A of the first lithium iron phosphate material. Optionally, the difference between B and A (ie, BA) is greater than 0.1 g / cm 3 At this time, it is more conducive for the first and second lithium iron phosphate materials to form a denser stack.

[0013] In some embodiments of the present application, the B is greater than 2.5 g / cm 3 Up to 2.6g / cm 3 In this case, the C can be greater than 2.6 g / cm 3 Up to 2.95g / cm 3 The a may be in the range of greater than or equal to 0.062 to less than 0.3225.

[0014] It should be noted that the maximum compaction density of a material mentioned in this application may refer to the maximum available compaction density of a positive electrode sheet made of the material, or the maximum compaction density obtained by testing the material with a powder compaction density meter.

[0015] Optionally, the D50 particle size of the first lithium iron phosphate material is in the range of 0.3 μm-0.70 μm. In this case, the lithium ion diffusion path of the small-particle lithium iron phosphate material is relatively small, which has better electrical performance for the manufactured battery.

[0016] Optionally, the D50 particle size of the second lithium iron phosphate material is in the range of 0.75 μm-1.5 μm. In this case, the lithium iron phosphate material with a large particle size can facilitate the improvement of the compaction density of the positive electrode material.

[0017] The D50 particle sizes of the two lithium iron phosphate materials are within the above range, and they can be closely packed by appropriately mixing the two lithium iron phosphate materials with large and small particle sizes, thereby improving the compaction density of the resulting positive electrode material.

[0018] In the present application, the surfaces of the first lithium iron phosphate material and the second lithium iron phosphate material have a carbon coating layer, which can be obtained by sequentially sand-milling, spray-drying and sintering a mixed slurry of a phosphorus source, an iron source (iron phosphate can also be used as both a phosphoric acid and an iron source), a lithium source and a carbon source. The present application does not limit the specific preparation methods of the two lithium iron phosphate materials.

[0019] The preparation method of the lithium iron phosphate positive electrode material provided in the first aspect of the present application can realize the controllable preparation of the compaction density of the lithium iron phosphate positive electrode material mixed by the two lithium iron phosphate materials, and then the electrochemical performance of the battery made by the positive electrode material is better. The preparation method is simple in process, easy to operate, and suitable for large-scale production.

[0020] The second aspect of the present application provides a positive electrode plate, which includes a positive electrode collector and a positive electrode material layer arranged on the surface of the positive electrode collector, and the positive electrode material layer includes a lithium iron phosphate positive electrode material prepared by the above method, a conductive agent and a binder.

[0021] The positive electrode material layer can be formed by coating a positive electrode slurry containing lithium iron phosphate positive electrode material, a conductive agent, a binder and a solvent on the positive electrode collector. Wherein, the solvent can be one or more of N-methylpyrrolidone (NMP), acetone and dimethylacetamide (DMAC). The positive electrode collector includes any one of aluminum foil, carbon-coated aluminum foil and perforated aluminum foil. Wherein, the conductive agent includes but is not limited to one or more of carbon nanotubes, graphene, carbon black and carbon fiber. The binder includes but is not limited to one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl alcohol (PVA), styrene-butadiene rubber (SBR), polyacrylic acid (PAA), polyacrylate, polyacrylonitrile (PAN), sodium carboxymethyl cellulose (CMC) and sodium alginate.

[0022] Optionally, the maximum compaction density of the positive electrode sheet is substantially consistent with the maximum compaction density C of the positive electrode material calculated according to the formula of the present application. Therefore, without making the positive electrode sheet from the positive electrode material mixed with the first and second lithium iron phosphate materials, the compaction density of the positive electrode sheet made of the positive electrode material can be accurately estimated according to the formula provided in the present application, which can save materials and time.

[0023] The third aspect of the present application provides a lithium-ion battery, which includes a positive electrode sheet, a negative electrode sheet, and an electrolyte and a separator located between the positive electrode sheet and the negative electrode sheet.

[0024] The lithium-ion battery using the above-mentioned positive electrode plate has a higher discharge specific capacity and a higher energy density. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a cross-sectional scanning electron microscope (SEM) photograph of the positive electrode sheet of Example 5 of the present application.

[0026] Figure 2 This is a cross-sectional SEM photograph of the positive electrode sheet of Comparative Example 1.

[0027] Figure 3 The cycle performance curves of the soft-pack batteries of Example 5 and Comparative Example 1 are shown. DETAILED DESCRIPTION

[0028] The following are exemplary embodiments of the present invention. It should be noted that a person skilled in the art may make several improvements and modifications without departing from the principles of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present invention.

[0029] The technical solution of the present application is described below in conjunction with a number of specific embodiments.

[0030] Example 1

[0031] A method for preparing a lithium iron phosphate positive electrode material comprises the following steps:

[0032] The first lithium iron phosphate material LFP-1 was selected and its maximum compaction density A=1.85g / cm 3 , D50 is about 0.3μm; the second lithium iron phosphate material LFP-2 is selected and its maximum compaction density B is 2.51g / cm 3 , D50 is about 0.88μm;

[0033] The LFP-1 material and LFP-2 are mixed in a mass ratio of a:b to obtain the lithium iron phosphate positive electrode material LFP-3; wherein, according to the above formula, the mass proportion of LFP-1 is a=0.315A-0.086B-0.25=0.118, b=1-a=0.882, and the fitting value of the maximum compaction density of the LFP-3 material is C=0.61+0.37A+0.546B=2.66g / cm 3 .

[0034] The positive electrode material LFP-3 is prepared into a positive electrode sheet: the LFP-3 material is mixed with a binder (specifically polyvinylidene fluoride, PVDF) and conductive carbon black in a mass ratio of 85:5:10, and an appropriate amount of N-methyl ketone pyrrole (NMP) is added thereto, and after mixing evenly, a positive electrode slurry is obtained; the positive electrode slurry is coated on both sides of the carbon-coated aluminum foil, and after drying, a surface density of 450g / m 2 The maximum compaction density of the positive electrode sheet was measured to be 2.66 g / cm 3 , which is consistent with the fitting value of the maximum compaction density of the positive electrode material LFP-3 calculated according to the formula of this application.

[0035] A lithium-ion battery was prepared by using a positive electrode sheet made of the positive electrode material LFP-3 prepared in Example 1 as a positive electrode, a graphite electrode sheet as a negative electrode, a polypropylene film as a separator, and a solution of ethylene carbonate (EC) containing 1.0 mol / L LiPF6 and dimethyl carbonate (DMC) = 1:1 (volume ratio) as an electrolyte, and assembled into a soft-pack battery in a dew point environment.

[0036] Example 2

[0037] A method for preparing a lithium iron phosphate positive electrode material, comprising:

[0038] The first lithium iron phosphate material LFP-1 was selected and its maximum compaction density A=2.03g / cm 3 , D50 is about 0.5μm; the second lithium iron phosphate material LFP-2 is selected and its maximum compaction density B is tested to be 2.55g / cm 3 , D50 is about 0.94μm;

[0039] The LFP-1 material and LFP-2 are mixed in a mass ratio of a:b to obtain the lithium iron phosphate positive electrode material LFP-3; wherein, according to the above formula, the mass proportion of LFP-1 is calculated as a=0.315A-0.086B-0.25=0.171, b=1-a=0.829, and the fitting value of the maximum compaction density of the LFP-3 material is C=0.61+0.37A+0.546B=2.75g / cm 3 The positive electrode material LFP-3 was made into a positive electrode sheet according to the method described in Example 1, and the actual value of its maximum compaction density was measured to be 2.76 g / cm 3 , which is very close to the fitted value.

[0040] According to the method described in Example 1, the positive electrode sheet made of the LFP-3 material of Example 2 was assembled into a soft-pack battery.

[0041] Example 3

[0042] A method for preparing a lithium iron phosphate positive electrode material, comprising:

[0043] The first lithium iron phosphate material LFP-1 was selected and its maximum compaction density A=2.45g / cm 3 , D50 is about 0.67μm; the second lithium iron phosphate material LFP-2 is selected and its maximum compaction density B is tested to be 2.58g / cm 3 , D50 about 1.2μm;

[0044] The LFP-1 material and LFP-2 are mixed in a mass ratio of a:b to obtain the lithium iron phosphate positive electrode material LFP-3; wherein, according to the above formula, the mass proportion of LFP-1 is calculated to be a=0.315A-0.086B-0.25=0.301, b=1-a=0.699, and the fitting value of the maximum compaction density of the LFP-3 material is C=0.61+0.37A+0.546B=2.93g / cm 3 The positive electrode material LFP-3 was made into a positive electrode sheet according to the method described in Example 1, and the actual value of its maximum compaction density was measured to be 2.93 g / cm 3 , which is consistent with the fitted value.

[0045] According to the method described in Example 1, the positive electrode sheet made of the LFP-3 material of Example 3 was assembled into a soft-pack battery.

[0046] Example 4

[0047] A method for preparing a lithium iron phosphate positive electrode material, comprising:

[0048] The first lithium iron phosphate material LFP-1 was selected and its maximum compaction density A=2.19g / cm 3 , D50 is about 0.55μm; the second lithium iron phosphate material LFP-2 is selected and its maximum compaction density B is tested to be 2.60g / cm 3 , D50 is about 1.4μm;

[0049] The LFP-1 material and LFP-2 are mixed in a mass ratio of a:b to obtain the lithium iron phosphate positive electrode material LFP-3; wherein, according to the above formula, the mass proportion of LFP-1 is a=0.315A-0.086B-0.25=0.217, b=1-a=0.783, and the fitting value of the maximum compaction density of the LFP-3 material is C=0.61+0.37A+0.546B=2.84g / cm 3 The positive electrode material LFP-3 was made into a positive electrode sheet according to the method described in Example 1, and the actual value of its maximum compaction density was measured to be 2.83 g / cm 3 , which is very close to the fitted value.

[0050] According to the method described in Example 1, the positive electrode sheet made of the LFP-3 material of Example 4 was assembled into a soft-pack battery.

[0051] Example 5

[0052] A method for preparing a lithium iron phosphate positive electrode material, comprising:

[0053] The first lithium iron phosphate material LFP-1 was selected and its maximum compaction density A=2.49g / cm 3 , D50 is about 0.7μm; the second lithium iron phosphate material LFP-2 is selected and its maximum compaction density B is 2.60g / cm 3 , D50 is about 1.4μm;

[0054] The LFP-1 material and LFP-2 are mixed in a mass ratio of a:b to obtain the lithium iron phosphate positive electrode material LFP-3; wherein, according to the above formula, the mass proportion of LFP-1 is calculated to be a=0.315A-0.086B-0.25=0.312, b=1-a=0.688, and the fitting value of the maximum compaction density of the LFP-3 material is C=0.61+0.37A+0.546B=2.95g / cm 3 The positive electrode material LFP-3 was made into a positive electrode sheet according to the method described in Example 1, and the actual value of its maximum compaction density was measured to be 2.96 g / cm 3 , which is very close to the fitted value.

[0055] According to the method described in Example 1, the positive electrode sheet made of the LFP-3 material of Example 5 was assembled into a soft-pack battery.

[0056] In order to highlight the beneficial effects of the present application, the following comparative examples 1-2 are provided.

[0057] Comparative Example 1 - Set up for Examples 4 and 5

[0058] A maximum compacted density of 2.60g / cm 3 According to the method described in Example 1, the material is made into a positive electrode sheet and assembled into a soft pack battery.

[0059] Comparative Example 2 - Setting for Example and 5

[0060] A positive electrode material is prepared by the following method:

[0061] The maximum compaction density is 2.49 g / cm 3 The lithium iron phosphate material has a maximum compaction density of 2.60g / cm 3 The lithium iron phosphate material is mixed in a mass ratio of 1:1 to obtain a positive electrode material, and the maximum compaction density of the positive electrode material is 2.53g / cm3 .

[0062] According to the method described in Example 1, the positive electrode material of Comparative Example 2 was made into a positive electrode sheet and assembled into a soft-pack battery.

[0063] Conventional lithium iron phosphate material, at 400g / m 2 At a surface density of 2.6 g / cm or higher, the electrode has a compaction density of up to 2.6 g / cm due to the unoptimized particle size distribution. 3 If the roller pressure is further increased to improve compaction, the particles will break and performance will be affected; or the pole pieces will break and become unusable, making it impossible to further increase the compaction density. Figure 1 , Figure 2 The following are cross-sectional SEM photos of the positive electrode sheets of Example 5 and Comparative Example 1 of the present application. Figure 1 and Figure 2 It can be seen from the comparison that in Comparative Example 1, since different lithium iron phosphate materials are not mixed, the pressure is reduced to 2.6 g / cm 3 After that, the particles are more broken (see Figure 2 In Example 5, since different lithium iron phosphate materials are mixed according to the method of the present application, the compaction density of the obtained positive electrode material reaches nearly 3.00 g / cm 3 There is still no obvious breakage of the positive electrode material particles.

[0064] In order to strongly support the beneficial effects of the present application, the soft-pack batteries of each embodiment and comparative example were subjected to cycle performance tests: 0.5C / 0.5C cycle tests were performed on each soft-pack battery at 25°C, with a voltage range of 2.0-3.8V. The cycle performance curves of the soft-pack batteries of Example 5 and Comparative Example 1 are as follows: Figure 3 The data of the first cycle coulombic efficiency and capacity retention rate of the batteries of various embodiments and comparative examples are summarized in the following Table 1.

[0065] Table 1

[0066]

[0067] Depend on Figure 3It can be seen from Table 1 that the battery of Comparative Example 1, which uses only one lithium iron phosphate material as the positive electrode material, is significantly inferior to the positive electrode material (Examples 4 and 5) obtained by combining different lithium iron phosphate materials in the manner provided in this application in terms of the first coulomb efficiency and cycle performance. In addition, from the comparison between Example 5 and Comparative Example 2 in Table 1, it can be seen that when the same two lithium iron phosphate materials are not mixed in the manner provided in this application, the compaction density of the obtained positive electrode material is low, and the electrochemical performance of the button battery prepared using the positive electrode material is also poor. It can be seen that the compaction density of the positive electrode sheet made of the positive electrode material obtained by the method of the embodiment of the present application is high, and the electrochemical performance of the button battery containing the positive electrode sheet is excellent, the discharge specific capacity is high, which is conducive to improving the battery energy density, and the cycle performance is excellent.

[0068] The above only expresses several exemplary embodiments of the present application, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present application. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present application, which all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be based on the attached claims.

Claims

1. A method for preparing a lithium iron phosphate positive electrode material, characterized in that: The following steps are involved: The first lithium iron phosphate material with a maximum compaction density of A and the second lithium iron phosphate material with a maximum compaction density of B are mixed at a mass ratio of a:b to obtain a lithium iron phosphate positive electrode material; Wherein, a=0.315A-0.086B-0.25, b=1-a; C = 0.61 + 0.37A + 0.546B; C represents the fitted value of the maximum compaction density of the lithium iron phosphate positive electrode material, and the units of A, B, and C are all g / cm 3 , the B is greater than 2.5g / cm 3 , the A is between 1.7 and 2.5 g / cm 3 The C is consistent with the maximum compaction density of the positive electrode sheet made of the lithium iron phosphate positive electrode material; wherein the lithium iron phosphate positive electrode material is made into a positive electrode sheet specifically as follows: the lithium iron phosphate positive electrode material is mixed with polyvinylidene fluoride and conductive carbon black in a mass ratio of 85:5:10, and N-methyl ketone pyrrole is added and mixed evenly to obtain a positive electrode slurry; the positive electrode slurry is coated on both sides of the carbon-coated aluminum foil, and after drying, a surface density of 450g / m 2 Double-sided positive electrode.

2. The preparation method according to claim 1, characterized in that The difference between B and A is greater than 0.1 g / cm 3 .

3. The preparation method according to claim 1, characterized in that: The B is greater than 2.5g / cm 3 Up to 2.6g / cm 3 within the range.

4. The preparation method according to any one of claims 1 to 3, characterized in that: The D50 particle size of the first lithium iron phosphate material is in the range of 0.3 μm-0.70 μm.

5. The preparation method according to any one of claims 1 to 3, characterized in that: The D50 particle size of the second lithium iron phosphate material is in the range of 0.75 μm-1.5 μm.

6. A positive electrode sheet, characterized in that: The positive electrode sheet contains a lithium iron phosphate positive electrode material prepared by the preparation method described in any one of claims 1-5.

7. A lithium ion battery, characterized in that: The lithium-ion battery comprises the positive electrode sheet according to claim 6.