A new lithium-boron material for thermal battery negative electrode and preparation method and thermal battery

CN115863646BActive Publication Date: 2024-11-153RD GENERAL DESIGN DEPT CHINA AEROSPACE SCI & IND CORP
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202211648035.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-21
Publication Date
2024-11-15
Estimated Expiration
2042-12-21

AI Technical Summary

Technical Problem

The thermal battery has low strength in the skeleton structure of lithium boron alloy in a large scale mechanical environment, and metal lithium is prone to spillover, resulting in a short circuit in direct contact between the negative electrode material and the positive electrode material, which is poor in safety.

Method used

Using new lithium boron materials, doping 0.5-5% stabilizer (such as alumina and magnesium oxide) and 0.3-5% conductive agent (such as graphite powder, iron powder) into the lithium boron alloy, and rolling pressure The process makes it evenly distributed, improves the skeleton strength and conductivity of the material, and reduces the spillover of metal lithium.

Benefits of technology

It improves the safety and conductivity of thermal batteries in a large-scale mechanical environment, avoids short-circuit failure between the negative electrode material and the positive electrode material, and extends the working time and capacity characteristics of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115863646B_ABST
    Figure CN115863646B_ABST
Patent Text Reader

Abstract

The present invention relates to a new type of lithium-boron material for the negative electrode of a thermal battery, a preparation method and a thermal battery, and belongs to the technical field of negative electrode materials for thermal batteries. It solves at least one of the problems in the prior art that when thermal batteries are in an external large-scale mechanical environment, the lithium-boron alloy skeleton structure has low strength, the metal lithium is easy to overflow, the negative electrode material and the positive electrode material are in direct contact and short circuit occurs, and the safety is poor. A new type of lithium-boron material for the negative electrode of a thermal battery, according to mass percentage, the material includes 0.5-5% of a stabilizer, 0.3-5% of a conductive agent, and the balance is a lithium-boron alloy. The thermal battery prepared using the new type of lithium-boron material described in the present invention has high safety in a large-scale mechanical environment, reduces the overflow of metal lithium in the negative electrode material, and avoids short circuit failure caused by direct contact with the positive electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thermal battery negative electrode materials, and in particular to a novel lithium-boron material for a thermal battery negative electrode, a preparation method and a thermal battery. Background Art

[0002] Thermal batteries are a type of primary battery that can be stored for a long time. Their working characteristics are that they have no load capacity when not activated. After receiving an external activation signal (electrical signal or mechanical force signal, etc.), the battery uses its own heating system to melt the internal solid salt electrolyte into a liquid state, and then has the load capacity. Thermal batteries have many advantages such as high specific power and specific energy, fast activation, wide operating temperature range, long storage life, maintenance-free, and strong environmental adaptability, and are widely used in various weapons and equipment.

[0003] Before activation, thermal batteries may be subjected to large mechanical vibrations, shocks or centrifugal accelerations during transportation, installation tests, etc. These mechanical environments may damage thermal batteries, especially their internal battery stacks, and affect the safety of battery use. In addition, according to the principle of thermal batteries, after the battery is activated, its interior is in a molten state and will be more susceptible to the impact of the mechanical environment. Current thermal battery technology is sufficient to meet safety requirements in conventional mechanical environments, but with the continuous improvement of weapon or aircraft performance and operating environment conditions, the mechanical environment that thermal batteries are subjected to is becoming more and more complex, which will place higher requirements on the mechanical resistance of thermal batteries.

[0004] In order to improve the mechanical resistance of thermal batteries, it is necessary to optimize and improve the materials of thermal batteries. The positive electrode materials commonly used in thermal batteries have high structural strength and poor fluidity, so they do not require special treatment to meet the stability requirements under large-scale mechanical environmental conditions; the electrolyte material can improve its mechanical stability by optimizing the performance and material ratio of the binder material to achieve the performance of large-scale mechanical environments. However, the optimization of negative electrode materials still needs to be studied. When thermal batteries are in an external large-scale mechanical environment, the lithium-boron alloy skeleton structure has low strength, metallic lithium is easy to overflow, the negative electrode material and the positive electrode material are in direct contact and short circuit occurs, and the safety is poor. Summary of the invention

[0005] In view of the above analysis, the embodiments of the present invention aim to provide a new lithium-boron material for the negative electrode of a thermal battery, a preparation method and a thermal battery, so as to solve at least one of the problems of the thermal battery in the prior art when it is in an external large-scale mechanical environment, such as low strength of the lithium-boron alloy skeleton structure, easy overflow of metallic lithium, short circuit caused by direct contact between the negative electrode material and the positive electrode material, and poor safety.

[0006] In a first aspect, a new lithium-boron material for a negative electrode of a thermal battery is provided. In terms of mass percentage, the material comprises 0.5-5% of a stabilizer, 0.3-5% of a conductive agent, and the remainder is a lithium-boron alloy.

[0007] Furthermore, the stabilizer is aluminum oxide and / or magnesium oxide.

[0008] Furthermore, the particle size of the stabilizer is 40 to 300 meshes.

[0009] Furthermore, the conductive agent is one or more of graphite powder, iron powder or cobalt powder.

[0010] Furthermore, the particle size of the conductive agent is 40 to 300 meshes.

[0011] Furthermore, the mass fraction of lithium in the lithium-boron alloy is 50-70%.

[0012] In a second aspect, a method for preparing the novel lithium-boron material for the negative electrode of a thermal battery is provided, wherein the method comprises the following steps:

[0013] (1) Weigh and set aside the raw materials according to the ratio of each raw material;

[0014] (2) placing the reserved lithium-boron alloy into a rolling mill for rolling to obtain a lithium-boron alloy strip, then evenly spreading a stabilizer and a conductive agent on the surface of the lithium-boron alloy strip, folding the strip in half, placing the strip into a rolling mill for further rolling, and repeating the rolling process 3-5 times;

[0015] (3) The rolling equipment is set to the required thickness to obtain the novel lithium-boron material for the negative electrode of the thermal battery.

[0016] Furthermore, the rolling in step (2) is performed in an environment with a humidity of ≤3%, and the thickness of the lithium-boron alloy strip is 0.5-5 mm and the width is 50-500 mm.

[0017] Furthermore, in step (2), the rolling pressure is 100-300 MPa and the temperature is 80-200°C.

[0018] In a third aspect, a thermal battery made from the lithium-boron material is provided.

[0019] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0020] (1) The novel lithium-boron material for the negative electrode of the thermal battery of the present invention is doped with a stabilizer to improve the skeleton strength of the lithium-boron material and the adsorption effect of metallic lithium, thereby reducing the overflow of metallic lithium in the negative electrode material and avoiding short circuit failure caused by direct contact with the positive electrode material, thereby improving the safety of the thermal battery under a large-scale mechanical environment. In addition, the conductivity of the lithium-boron material is ensured by doping with a conductive agent.

[0021] (2) In the present invention, the stabilizer and the conductive agent are doped at a specific ratio. This is because the higher the doping ratio of the stabilizer, the less the metallic lithium overflows from the lithium-boron alloy, and the more obvious the stabilization effect. However, the higher the doping ratio, the less the content of active metallic lithium, resulting in a shorter battery working time. The more the conductive agent is doped, the less the content of active metallic lithium, which affects the capacity characteristics of the negative electrode material and shortens the battery working time.

[0022] (3) The stabilizer and the conductive agent in the present invention are selected with a specific mesh size. This is because the smaller the stabilizer particle size, the less the metallic lithium overflows from the lithium-boron alloy, and the more obvious the stabilization effect. However, after the stabilizer particle size reaches 300 meshes, the effect of suppressing the overflow by further reducing the particle size is not obvious. At the same time, when the stabilizer particle size is about 170 meshes, the battery working time is the longest, and the capacity characteristics of the lithium-boron alloy negative electrode material are the best. The larger the stabilizer particle size, the more obvious the overflow, the loss of active metallic lithium, and the shorter the working time; the smaller the stabilizer particle size, the stronger the adsorption capacity of metallic lithium, and the limited active metallic lithium participates in the reaction, resulting in a shorter working time; the smaller the conductive agent particle size, the smaller the battery internal resistance, and accordingly, the longer the battery working time. When the particle size is greater than 300 meshes, the internal resistance decreases and tends to stabilize.

[0023] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.

[0025] Figure 1 This is a photo of a battery stack of a thermal battery made of lithium-boron material prepared in Example 1 of the present invention after working in a large-scale force environment;

[0026] Figure 2 This is a photo of a battery stack of a thermal battery made of lithium-boron material prepared in Comparative Example 1 of the present invention after working in a large-scale force environment;

[0027] Figure 3 It is a large-scale mechanical vibration spectrum in the present invention. DETAILED DESCRIPTION

[0028] The preferred embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of this application and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.

[0029] A specific embodiment of the present invention discloses a novel lithium-boron material for a negative electrode of a thermal battery. In terms of mass percentage, the material includes 0.5-5% of a stabilizer, 0.3-5% of a conductive agent, and the remainder is a lithium-boron alloy.

[0030] Exemplarily, the stabilizer is 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0% and the conductive agent is 0.3%, 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%.

[0031] Compared with the prior art, the thermal battery negative electrode of the present embodiment uses a new type of lithium-boron material doped with a stabilizer to improve the skeleton strength of the lithium-boron material and the adsorption effect on metallic lithium, thereby reducing the overflow of metallic lithium in the negative electrode material and avoiding short-circuit failure caused by direct contact with the positive electrode material, thereby improving the safety of the thermal battery in a large-scale mechanical environment. In addition, the conductivity of the lithium-boron material is ensured by doping with a conductive agent.

[0032] In a further preferred embodiment, the material includes, by mass percentage, 1-1.5% of a stabilizer, 2-3% of a conductive agent, and the remainder is a lithium-boron alloy.

[0033] It should be noted that, under the above-mentioned ratio, the lithium-boron alloy can ensure low internal resistance while having sufficient stability to ensure the safety of the thermal battery.

[0034] Specifically, the stabilizer is aluminum oxide and / or magnesium oxide.

[0035] In the present invention, the skeleton strength of the lithium-boron material is improved by doping a stabilizer, the overflow of metallic lithium is reduced, short-circuit failure caused by direct contact with the positive electrode material is avoided, and the safety of the thermal battery under large-scale mechanical environmental conditions is improved.

[0036] Specifically, the particle size of the stabilizer is 40 to 300 meshes.

[0037] Exemplarily, the particle size of the stabilizer is 40 mesh, 60 mesh, 80 mesh, 100 mesh, 120 mesh, 140 mesh, 160 mesh, 180 mesh, 200 mesh, 220 mesh, 240 mesh, 260 mesh, 280 mesh, or 300 mesh.

[0038] In a further preferred embodiment, the particle size of the stabilizer is 80-200 mesh.

[0039] The stabilizer lithium ions with a specific particle size used in the present invention can reduce the flow of lithium atoms at high temperatures, play a role in adsorbing metal lithium atoms, improve safety, and ensure the conductivity of the negative electrode material. When the stability particle size is 80-200 mesh, it can be ensured that the stabilizer has sufficient adsorption capacity for metal lithium.

[0040] Specifically, the conductive agent is one or more of graphite powder, iron powder or cobalt powder.

[0041] Where instructions are required, the particle size of the conductive agent is 40 to 300 meshes.

[0042] Exemplarily, the particle size of the conductive agent is 40 mesh, 60 mesh, 80 mesh, 100 mesh, 120 mesh, 140 mesh, 160 mesh, 180 mesh, 200 mesh, 220 mesh, 240 mesh, 260 mesh, 280 mesh, or 300 mesh.

[0043] In a further preferred embodiment, the particle size of the conductive agent is 80 to 200 meshes.

[0044] Since the addition of the stabilizer will reduce the conductivity of the negative electrode material, in order not to affect the conductivity, the particle size and ratio of the conductive agent of the present invention can keep the conductivity of the negative electrode material from being reduced. Adding too much conductive agent will affect the capacity of the battery. Therefore, the specific proportion of the conductive agent of the present invention can simultaneously meet the conductivity of the negative electrode material and does not affect the capacity of the battery. When the particle size of the conductive agent is 80 to 200 meshes, it can be ensured that the conductive agent can be more fully embedded in the lithium-boron alloy, thereby reducing the internal resistance of the negative electrode material.

[0045] It should be noted that the lithium-boron alloy is a strip with a thickness of 0.5 to 5 mm and a width of 50 to 500 mm, and the mass fraction of lithium in the lithium-boron alloy is 50 to 70%.

[0046] Exemplarily, the lithium-boron alloy has a thickness of 0.5 mm, 1.0 mm, 1.5 mm, 2.0 mm, 2.5 mm, 3.0 mm, 3.5 mm, 4.0 mm, 4.5 mm, and 5.0 mm, and a width of 50 mm, 100 mm, 150 mm, 200 mm, 250 mm, 300 mm, 350 mm, 400 mm, 450 mm, and 500 mm, and the mass fraction of lithium in the lithium-boron alloy is 50%, 55%, 60%, 65%, and 70%.

[0047] In a second aspect, a method for preparing the novel lithium-boron material for the negative electrode of a thermal battery is provided, wherein the method comprises the following steps:

[0048] (1) Weigh and set aside the raw materials according to the ratio of each raw material;

[0049] (2) placing the reserved lithium-boron alloy into a rolling mill for rolling to obtain a lithium-boron alloy strip, and then evenly spreading a stabilizer and a conductive agent on the surface of the lithium-boron alloy strip, folding the strip in half, placing the strip into a rolling mill for further rolling, and repeating the rolling process 3-5 times to ensure that the stabilizer and the conductive agent are evenly distributed in the lithium-boron alloy;

[0050] (3) The rolling equipment is set to the required thickness to obtain the novel lithium-boron material for the negative electrode of the thermal battery. It should be noted that the rolling in step (2) is carried out in an environment with a humidity of ≤3% to prevent the lithium-boron from absorbing water and deteriorating. The thickness of the lithium-boron alloy strip is 0.5-5 mm and the width is 50-500 mm.

[0051] It should be noted that in step (2), the rolling pressure is 100-300 MPa and the temperature is 80-200°C.

[0052] Exemplarily, the rolling pressure is 100MPa, 120MPa, 140MPa, 160MPa, 180MPa, 200MPa, 220MPa, 240MPa, 260MPa, 280MPa, 300MPa, 320MPa, 340MPa, 360MPa, 380MPa, 400MPa, and the temperature is 80°C, 100°C, 120°C, 140°C, 160°C, 180°C, 200°C.

[0053] By adopting the above-mentioned pressure and temperature, the lithium-boron alloy strip can be made soft, which is convenient for rolling forming.

[0054] In a third aspect, a thermal battery made of the new lithium-boron material used as the thermal battery negative electrode is provided.

[0055] The novel lithium-boron material for the negative electrode of the thermal battery of the present invention is further explained below through specific examples.

[0056] Example 1

[0057] A new lithium-boron material for a negative electrode of a thermal battery in this embodiment includes, by mass percentage, 2.5% of a stabilizer, 2.6% of a conductive agent, and the remainder is a lithium-boron alloy;

[0058] The stabilizer is magnesium oxide with a particle size of 170 meshes, the conductive agent is graphite powder with a particle size of 170 meshes, and the mass fraction of lithium in the lithium-boron alloy is 60%.

[0059] The method for preparing the novel lithium-boron material for the negative electrode of the thermal battery described in this embodiment comprises the following steps:

[0060] (1) Weigh and set aside the raw materials according to the ratio of each raw material;

[0061] (2) placing the reserved lithium-boron alloy into a rolling mill for rolling to obtain a lithium-boron alloy strip having a thickness of 0.6 mm and a width of 75 mm, and then evenly spreading a stabilizer and a conductive agent on the surface of the lithium-boron alloy strip, folding the strip in half, placing the strip into a rolling mill for further rolling, and repeating the rolling process 3-5 times. The rolling process is performed in an environment with a humidity of ≤3%, a rolling pressure of 100 MPa, and a temperature of 200° C.;

[0062] (3) The rolling equipment is set to the required thickness to obtain the novel lithium-boron material for the negative electrode of the thermal battery.

[0063] The thickness of the new lithium-boron material used for the negative electrode of the thermal battery in this embodiment is 0.5 mm.

[0064] The novel lithium-boron material prepared in this embodiment is punched into discs and used as negative electrode materials to assemble a thermal battery. Figure 3 The discharge test was carried out under the mechanical environment conditions described above. After the discharge, the battery was dissected and the shape of the battery stack was as follows: Figure 1 shown.

[0065] Example 2

[0066] A new lithium-boron material for a negative electrode of a thermal battery in this embodiment includes, by mass percentage, 0.5% of a stabilizer, 0.3% of a conductive agent, and the remainder is a lithium-boron alloy;

[0067] The stabilizer is aluminum oxide, and the particle size of the aluminum oxide is 40 meshes. The conductive agent is a mixture of graphite powder and iron powder in a ratio of 1:1, and the particle sizes of the graphite powder and the iron powder are both 40 meshes. The mass fraction of lithium in the lithium-boron alloy is 58%. The preparation method of the new lithium-boron material for the negative electrode of the thermal battery described in this embodiment comprises the following steps:

[0068] (1) Weigh and set aside the raw materials according to the ratio of each raw material;

[0069] (2) placing the reserved lithium-boron alloy into a rolling mill for rolling to obtain a lithium-boron alloy strip having a thickness of 0.5 mm and a width of 60 mm, and then evenly sprinkling a stabilizer and a conductive agent on the surface of the lithium-boron alloy strip, folding the strip in half, placing the strip into a rolling mill for further rolling, and repeating the rolling process 3-5 times. The rolling process is performed in an environment with a humidity of ≤3%, a rolling pressure of 200 MPa, and a temperature of 140° C.;

[0070] (3) The rolling equipment is set to the required thickness to obtain the novel lithium-boron material for the negative electrode of the thermal battery.

[0071] The thickness of the new lithium-boron material used for the negative electrode of the thermal battery in this embodiment is 0.5 mm.

[0072] Example 3

[0073] A new lithium-boron material for a negative electrode of a thermal battery in this embodiment includes, by mass percentage, 5% of a stabilizer, 5% of a conductive agent, and the remainder is a lithium-boron alloy;

[0074] The stabilizer is a mixture of magnesium oxide and aluminum oxide in a mass ratio of 1:1, the particle sizes of magnesium oxide and aluminum oxide are both 300 meshes, the conductive agent is iron powder, the particle size of graphite powder is 300 meshes, and the mass fraction of lithium in the lithium-boron alloy is 62%.

[0075] The method for preparing the novel lithium-boron material for the negative electrode of the thermal battery described in this embodiment comprises the following steps:

[0076] (1) Weigh and set aside the raw materials according to the ratio of each raw material;

[0077] (2) placing the reserved lithium-boron alloy into a rolling mill for rolling to obtain a lithium-boron alloy strip having a thickness of 0.8 mm and a width of 100 mm, and then evenly spreading a stabilizer and a conductive agent on the surface of the lithium-boron alloy strip, folding the strip in half, and placing the strip into a rolling mill for further rolling. Repeating the rolling process 3-5 times, the rolling is performed in an environment with a humidity of ≤3%, a rolling pressure of 300 MPa, and a temperature of 200° C.;

[0078] (3) The rolling equipment is set to the required thickness to obtain the novel lithium-boron material for the negative electrode of the thermal battery.

[0079] The thickness of the new lithium-boron material used for the negative electrode of the thermal battery in this embodiment is 0.5 mm.

[0080] Comparative Example 1

[0081] This comparative example uses the lithium-boron alloy of Example 1 (lithium-boron material without adding stabilizer and conductive agent) as the negative electrode material to assemble a thermal battery, and Figure 3 The discharge test was carried out under the mechanical environment conditions described above. After the discharge, the battery was dissected and the shape of the battery stack was as follows: Figure 2 shown.

[0082] from Figure 2 It can be seen from the figure that when lithium-boron material without stabilizer and conductive agent is used as negative electrode, metallic lithium overflows and contacts positive electrode material under the same mechanical environment, causing internal short circuit failure of the battery stack. Figure 1 It can be seen that when the new lithium-boron material prepared in Example 1 is used as the negative electrode, the stack morphology can still be well maintained, and there is no obvious overflow of metallic lithium in the negative electrode material, which ensures the safety of the thermal battery working in a large-scale mechanical environment.

[0083] Comparative Example 2

[0084] The preparation method of the lithium boron material in this comparative example is the same as that in Example 1, except that no stabilizer is added.

[0085] Comparative Example 3

[0086] The preparation method of the lithium boron material in this comparative example is the same as that in Example 1, except that no conductive agent is added.

[0087] Test Example 1

[0088] Only the particle size of the stabilizer was changed, and the other conditions were the same as in Example 1 to prepare the lithium-boron material. The lithium-boron material was punched into discs and used as the negative electrode material to assemble a thermal battery. The overflow of metallic lithium in the thermal battery was investigated. The specific method was the same as in Example 1. The results are shown in Table 1.

[0089] Table 1

[0090] Stabilizer particle size (mesh) Metal lithium spillover ratio (%) Working time(s) 30 8.03 351 40 7.97 356 170 3.26 403 300 3.01 373 310 3.01 369

[0091] It can be seen from the test results in Table 1 that when other conditions are the same, the smaller the particle size of the stabilizer, the less metal lithium overflows from the lithium-boron alloy, and the more obvious the stabilization effect. However, after the particle size reaches 300 mesh, the effect of reducing the particle size to suppress overflow is not obvious. At the same time, when the particle size is about 170 mesh, the battery working time is the longest, and the capacity characteristics of the lithium-boron alloy negative electrode material are the best. The larger the particle size, the more obvious the overflow, the loss of active metal lithium, and the shorter the working time; the smaller the particle size, the stronger the adsorption capacity of metal lithium, and the limited active metal lithium participates in the reaction, resulting in a shorter working time. Considering the overflow of metal lithium and the working time, the present invention selects a stabilizer with a particle size of 40-300 mesh.

[0092] Test Example 2

[0093] Only the doping ratio of the stabilizer was changed, and the other aspects were the same as in Example 1 to prepare the lithium-boron material. The lithium-boron material was punched into discs and used as the negative electrode material to assemble a thermal battery. The overflow of metallic lithium in the thermal battery was investigated. The specific method was the same as in Example 1. The results are shown in Table 2.

[0094] Table 2

[0095] Stabilizer doping ratio (%) Metal lithium spillover ratio (%) Working time(s) 0.4 9.54 364 0.5 3.54 395 2.7 3.25 377 5.0 2.95 335 5.1 2.88 330

[0096] It can be seen from the test results in Table 2 that when other conditions are the same, the higher the doping ratio of the stabilizer, the less the metallic lithium overflows from the lithium-boron alloy, and the more obvious the stabilization effect. However, the higher the ratio, the less the content of active metallic lithium, resulting in a shorter working time of the battery. Considering the metallic lithium overflow and the working time comprehensively, the doping ratio of the stabilizer in the present invention is 0.5-5.0%.

[0097] Test Example 3

[0098] Only the conductive particle size was changed, and the lithium-boron material was prepared in the same manner as in Example 1. The lithium-boron material was punched into discs and used as negative electrode materials to assemble a thermal battery. The internal resistance characteristics of the thermal battery were examined, as shown in Table 3.

[0099] Table 3

[0100] Conductive agent particle size (mesh) Internal resistance(Ω) Working time(s) 30 0.225 375 40 0.213 373 170 0.121 397 300 0.095 405 310 0.095 409

[0101] It can be seen from Table 3 that when other conditions are the same, the smaller the particle size of the conductive agent, the smaller the internal resistance of the battery, and correspondingly, the longer the working time of the battery. When the particle size is greater than 300 mesh, the internal resistance decreases and tends to stabilize. In the present invention, the particle size of the conductive agent is selected to be 40-300 mesh based on the internal resistance and working time of the thermal battery.

[0102] Test Example 4

[0103] Only the doping ratio of the conductive agent was changed, and the other aspects were the same as in Example 1 to prepare the lithium-boron material. The lithium-boron material was punched into discs and used as the negative electrode material to assemble a thermal battery, and the internal resistance characteristics of the thermal battery were examined, as shown in Table 4.

[0104] Table 4

[0105] Conductive agent doping ratio (%) Internal resistance(Ω) Working time(s) 0.4 0.234 366 0.5 0.223 365 2.7 0.121 393 5.0 0.088 375 5.1 0.089 369

[0106] It can be seen from Table 4 that when other conditions are the same, the more conductive agent is doped, the less active metal lithium content is, which affects the capacity characteristics of the negative electrode material and shortens the battery working time. Considering the internal resistance and battery working time, the conductive agent doping ratio is selected to be 0.5-5.0%.

[0107] Test Example 5

[0108] The lithium boron materials prepared in Example 1 and Comparative Examples 2-3 were punched into discs and used as negative electrode materials to assemble thermal batteries. The internal resistance characteristics of the thermal batteries were examined, as shown in Table 5.

[0109] Table 5

[0110] Group Internal resistance(Ω) Working time(s) Example 1 0.125 375 Comparative Example 2 Battery leakage -- Comparative Example 3 0.303 327

[0111] It can be seen from Table 5 that when no stabilizer is added, the battery leaks, and when no conductive agent is added, the internal resistance of the thermal battery is large and the working time is short.

[0112] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A new lithium-boron material for thermal battery negative electrode, characterized in that: According to mass percentage, the material includes 0.5-5% stabilizer, 0.3-5% conductive agent, and the balance is lithium-boron alloy; The stabilizer is aluminum oxide and / or magnesium oxide, and the particle size of the stabilizer is 40-300 meshes.

2. The novel lithium-boron material for thermal battery negative electrode according to claim 1, characterized in that: The conductive agent is one or more of graphite powder, iron powder or cobalt powder.

3. The novel lithium-boron material for thermal battery negative electrode according to claim 1 or 2, characterized in that: The particle size of the conductive agent is 40-300 meshes.

4. The novel lithium-boron material for thermal battery negative electrode according to claim 1 or 2, characterized in that: The mass fraction of lithium in the lithium-boron alloy is 50-70%.

5. A method for preparing a novel lithium-boron material for a negative electrode of a thermal battery according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: (1) Weigh and set aside the raw materials according to the ratio; (2) placing the reserved lithium-boron alloy into a rolling mill for rolling to obtain a lithium-boron alloy strip, and then evenly spreading a stabilizer and a conductive agent on the surface of the lithium-boron alloy strip, folding it in half, placing it into the rolling mill for further rolling, and repeating the rolling process 3-5 times; (3) The rolling equipment is set to the required thickness to obtain the new lithium-boron material for the negative electrode of the thermal battery.

6. The preparation method according to claim 5, characterized in that: The rolling in step (2) is carried out in an environment with a humidity of ≤3%, and the thickness of the lithium-boron alloy strip is 0.5-5 mm and the width is 50-500 mm.

7. The preparation method according to claim 5, characterized in that: In step (2), the rolling pressure is 100-300 MPa and the temperature is 80-200°C.

8. A thermal battery made of the lithium-boron material according to any one of claims 1 to 4 or the lithium-boron material prepared by the method according to any one of claims 5 to 7.

Citation Information

Cited By

  • High-energy lithium-boron alloy negative electrode

    CN117497694A