A sealant for the bottom of a vertical anti-seepage curtain and a preparation method thereof

By using sealants with components such as clay, sodium bentonite, barite powder, sodium pentasilate, carboxymethylcellulose and polyacrylamide, the problem of leakage at the bottom of the curtain is solved, improving the anti-seepage performance and reducing the Cost, effective sealing of pollutants is achieved.

CN115872720BActive Publication Date: 2024-11-26NORTH CHINA ENGINEERING INVESTIGATION INSTITUTE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211527915.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-30
Publication Date
2024-11-26
Estimated Expiration
2042-11-30

AI Technical Summary

Technical Problem

There is a leakage problem at the bottom of the curtain of the existing vertical anti-seepage system, which causes solid waste to pollute the downstream environment. The existing sealant preparation cost is high and the impermeability resistance is insufficient.

Method used

Using sealants with components such as clay, sodium bentonite, barite powder, sodium pentahydrate, carboxymethylcellulose and polyacrylamide, synergistically block the conduction by increasing density, fluidity, viscosity and dispersion. Water channels to reduce production costs.

Benefits of technology

It improves the anti-seepage performance of the sealant, reduces production costs, and effectively prevents pollutants from contaminating downstream through the bottom of the curtain, maintaining good water barrier performance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the field of environmental geotechnical engineering technology, and specifically discloses a sealant for the bottom of a vertical anti-seepage curtain and a preparation method thereof. The solid component of the sealant for the bottom of a vertical anti-seepage curtain is composed of the following raw materials in weight percentage: 68-75% clay, 15-20% sodium bentonite, 5-10% barite powder, 0.5-1.0% sodium silicate pentahydrate, 0.1-0.2% carboxymethyl cellulose and 0.8-1.0% polyacrylamide. The sealant for the bottom of a vertical anti-seepage curtain provided by the present invention improves the anti-seepage performance of the sealant and reduces the production cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of environmental geotechnical engineering, and in particular to a sealant used for the bottom of a vertical anti-seepage curtain and a preparation method thereof. Background Art

[0002] Landfill treatment is a commonly used method for domestic and industrial solid waste disposal at home and abroad. A vertical anti-seepage system is established around the landfill, that is, a vertical anti-seepage curtain is established on the impermeable layer, which can control the landfill solid waste within the landfill and prevent the surrounding groundwater from flowing into the landfill.

[0003] At present, the vertical anti-seepage system has the problem of leakage at the bottom of the curtain, which causes solid waste to pollute the downstream environment of the curtain. Therefore, it is often necessary to add sealants to completely seal the bottom of the curtain with the waterproof layer to block the migration of pollutants from the bottom of the curtain. Some studies have used modified bentonite and clay as raw materials to prepare sealants, but the weight percentage of modified bentonite is as high as 60-80%, and clay is only 20-40%. The manufacturing cost of the sealant is high, and its anti-seepage performance needs to be further improved. There are also studies that prepare shielding materials by mixing bentonite, kaolin, attapulgite, sodium carbonate, sodium silicate, sodium dodecyl sulfate, sodium hydroxide, sodium sulfate, magnesium oxide, calcium oxide, calcium sulfate, blast furnace slag, fly ash, red mud, mine tailings, phosphogypsum powder and water. There are many components involved and the cost is high, and its anti-seepage performance also needs to be further improved. Summary of the invention

[0004] In view of the above problems, the present invention provides a sealant for the bottom of a vertical anti-seepage curtain and a preparation method thereof, which improves the anti-seepage performance of the sealant and reduces the production cost.

[0005] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:

[0006] A sealant for the bottom of a vertical anti-seepage curtain is prepared by mixing the following raw materials in percentage by weight: 68-75% clay, 15-20% sodium bentonite, 5-10% barite powder, 0.5-1.0% sodium silicate pentahydrate, 0.1-0.2% carboxymethyl cellulose and 0.8-1.0% polyacrylamide.

[0007] Compared with the prior art, the sealant provided by the present invention for the bottom of the vertical anti-seepage curtain has clay as the main component, which reduces the production cost while maintaining good water-proof performance; the density of the sealant is increased by adding barite powder, so that the sealant is gradually accumulated from the bottom of the curtain upward, which promotes the sealant to fill the bottom of the curtain and the surrounding soil or rock cracks; the fluidity of the sealant is enhanced by adding sodium silicate pentahydrate, and the ability of the sealant to fill small cracks and voids is increased; by adding polyacrylamide, the sealant absorbs water and swells to block the space that is not completely filled, which can effectively reduce the tiny channels in the rock formation and soil; by adding carboxymethyl cellulose, the viscosity of the sealant is increased, making it difficult to disperse in water, and better maintaining the integrity of the sealant; through the interaction between carboxymethyl cellulose, sodium silicate pentahydrate and sodium bentonite, the interlayer spacing of sodium bentonite can be increased, and the dispersibility and stability of sodium bentonite can be further increased; through the synergistic effect of each component, the water guide channels on both sides of the bottom of the curtain can be blocked to prevent pollutants in the anti-seepage system from passing through the bottom of the curtain to pollute the downstream. The sealant used for the bottom of the vertical anti-seepage curtain provided by the present invention improves the anti-seepage performance of the sealant and reduces the production cost.

[0008] Preferably, the sealant is a slurry, which further comprises water, wherein the weight ratio of water to the solid component is 3:6.5 to 3:7.5.

[0009] Preferably, the permeability coefficient of the clay is ≤10 -8 cm / s, plasticity index I P ≥17. The performance of the final sealant is guaranteed by limiting the permeability coefficient and plasticity index of the clay; at the same time, the present invention can use local clay as the main component, reducing the purchase and transportation costs of materials, thereby reducing the overall production cost.

[0010] Preferably, the permeability coefficient of the sodium bentonite is ≤10 -9 cm / s.

[0011] Preferably, the particle size of the barite powder is in the range of 0.05 to 0.10 mm.

[0012] Preferably, the viscosity of the carboxymethyl cellulose is 800-1500 mPa·s.

[0013] The present invention also provides a method for preparing the sealant for the bottom of the vertical anti-seepage curtain, comprising the following steps:

[0014] S1, adding clay to water and stirring for 3 to 5 minutes to obtain a first mixed slurry;

[0015] S2, adding sodium bentonite to the first mixed slurry and stirring for 2 to 3 minutes to obtain a second mixed slurry;

[0016] S3, adding barite powder, sodium silicate pentahydrate, carboxymethyl cellulose and polyacrylamide to the second mixed slurry respectively, stirring for 3 to 5 minutes, and obtaining a sealant for the bottom of the vertical anti-seepage curtain.

[0017] The present invention sequentially adds clay, sodium bentonite, barite powder, sodium silicate pentahydrate, carboxymethyl cellulose and polyacrylamide into water, so that the components can fully interact with each other to form a uniform viscous slurry, and give full play to the synergistic effect of the components.

[0018] Preferably, in steps S1 to S3, the stirring speed is 1200 to 1500 r / min. DETAILED DESCRIPTION

[0019] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0020] In order to better illustrate the present invention, further examples are given below.

[0021] The clay selected in the embodiments and comparative examples of the present invention is clay from Qianshan County, Shangrao, Jiangxi Province (specific location), and the permeability coefficient of the clay is 9.3×10 -8 cm / s, plasticity index I P is 19; the permeability coefficient of the selected sodium bentonite is 8.5×10 -10 cm / s; the particle size range of the selected barite powder is 0.08 mm; the viscosity of the selected carboxymethyl cellulose is 1200 mPa·s.

[0022] Example 1

[0023] (1) Add 400 g of water to a forced mixer, then add 680 g of local clay, and stir at a speed of 1200 r / min for 3 min. Then add 200 g of sodium bentonite, and continue stirring at the current speed for 2 min. Finally, add 100 g of barite powder, 10 g of sodium silicate pentahydrate, 2 g of carboxymethyl cellulose, and 8 g of polyacrylamide, respectively, and continue stirring at the current speed for 3 min to obtain a prepared sealant for the bottom of a vertical anti-seepage curtain.

[0024] (2) According to the variable head permeability test test of GB / T 50123-2019 "Standard for Geotechnical Test Methods", the permeability coefficient of the sealant in this embodiment is 8.9×10 -10 cm / s.

[0025] Example 2

[0026] (1) Add 460 g of water to a forced mixer, then add 750 g of local clay, and stir at a speed of 1500 r / min for 5 min. Then add 150 g of sodium bentonite, and continue stirring at the current speed for 3 min. Finally, add 84 g of barite powder, 5 g of sodium silicate pentahydrate, 1 g of carboxymethyl cellulose, and 10 g of polyacrylamide, respectively, and continue stirring at the current speed for 5 min to obtain a prepared sealant for the bottom of a vertical anti-seepage curtain.

[0027] (2) According to the variable head permeability test test of GB / T 50123-2019 "Standard for Geotechnical Test Methods", the permeability coefficient of the sealant in this embodiment is 6.2×10 -10 cm / s.

[0028] Example 3

[0029] (1) Add 430 g of water to a forced mixer, then add 700 g of local clay, and stir at a speed of 1300 r / min for 4 min. Then add 180 g of sodium bentonite, and continue stirring at the current speed for 3 min. Finally, add 100 g of barite powder, 9 g of sodium silicate pentahydrate, 2 g of carboxymethyl cellulose, and 9 g of polyacrylamide, respectively, and continue stirring at the current speed for 4 min to obtain a prepared sealant for the bottom of a vertical anti-seepage curtain.

[0030] (2) According to the variable head permeability test test of GB / T 50123-2019 "Standard for Geotechnical Test Methods", the permeability coefficient of the sealant in this embodiment is 5.4×10 -10 cm / s.

[0031] Example 4

[0032] (1) Add 430 g of water to a forced mixer, then add 720 g of local clay, and stir at a speed of 1300 r / min for 4 min. Then add 180 g of sodium bentonite, and continue stirring at the current speed for 3 min. Finally, add 82 g of barite powder, 7.5 g of sodium silicate pentahydrate, 1.5 g of carboxymethyl cellulose, and 9 g of polyacrylamide, respectively, and continue stirring at the current speed for 4 min to obtain a prepared sealant for the bottom of a vertical anti-seepage curtain.

[0033] (2) According to the variable head permeability test test of GB / T 50123-2019 "Standard for Geotechnical Test Methods", the permeability coefficient of the sealant in this embodiment is 2.3×10 -10 cm / s.

[0034] Comparative Example 1

[0035] (1) In this comparative example, 360 g of clay and 540 g of sodium bentonite were added, and the addition amounts and preparation methods of the remaining components were the same as those in Example 4 to prepare a sealant for the bottom of a vertical anti-seepage curtain.

[0036] (2) According to the variable head permeability test test of GB / T 50123-2019 "Standard for Geotechnical Test Methods", the permeability coefficient of the sealant in this embodiment is 7.8×10 -9 cm / s.

[0037] Comparative Example 2

[0038] (1) In this comparative example, carboxymethyl cellulose was not added, and the addition amounts of the remaining components and the preparation methods were the same as those in Example 4 to prepare a sealant for the bottom of a vertical anti-seepage curtain.

[0039] (2) According to the variable head permeability test test of GB / T 50123-2019 "Standard for Geotechnical Test Methods", the permeability coefficient of the sealant in this embodiment is 6.2×10 -9 cm / s.

[0040] Comparative Example 3

[0041] (1) In this comparative example, sodium silicate pentahydrate was not added, and the addition amounts and preparation methods of the remaining components were the same as those in Example 4 to prepare a sealant for the bottom of a vertical anti-seepage curtain.

[0042] (2) According to the variable head permeability test test of GB / T 50123-2019 "Standard for Geotechnical Test Methods", the permeability coefficient of the sealant in this embodiment is 1.3×10 -9 cm / s.

[0043] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A sealant for the bottom of a vertical anti-seepage curtain, characterized in that: The sealant is made of the following raw materials in percentage by weight: 68-75% clay, 15-20% sodium bentonite, 5-10% barite powder, 0.5-1.0% sodium silicate pentahydrate, 0.1-0.2% carboxymethyl cellulose and 0.8-1.0% polyacrylamide; The permeability coefficient of the sodium bentonite is ≤10 -9 cm / s; The particle size range of the barite powder is 0.05-0.10 mm; The viscosity of the carboxymethyl cellulose is 800-1500 mPa·s; The sealant is a slurry, which also includes water, wherein the weight ratio of water to solid components is 3:6.5 to 3:7.5; The preparation method of the sealant for the bottom of the vertical anti-seepage curtain comprises the following steps: S1, adding clay to water and stirring for 3-5 minutes to obtain a first mixed slurry; S2, adding sodium bentonite to the first mixed slurry and stirring for 2-3 minutes to obtain a second mixed slurry; S3, adding barite powder, sodium silicate pentahydrate, carboxymethyl cellulose and polyacrylamide to the second mixed slurry respectively, and stirring for 3 to 5 minutes to obtain a sealant for the bottom of the vertical anti-seepage curtain; The clay, the sodium bentonite, the barite powder, the sodium silicate pentahydrate, the carboxymethyl cellulose and the polyacrylamide are sequentially added into water.

2. The sealant for the bottom of a vertical anti-seepage curtain according to claim 1, characterized in that: The permeability coefficient of the clay is ≤10 -8 cm / s, plasticity index IP≥17.

3. The sealant for the bottom of a vertical anti-seepage curtain according to claim 1, characterized in that: In steps S1 to S3, the stirring speed is 1200 to 1500 r / min.