A preparation method of lithium iron phosphate positive electrode material, positive electrode sheet and lithium ion battery
By regulating the sintering temperature and time of lithium iron phosphate materials, and combining spherical and irregular morphology materials, the compaction density of the cathode material is increased, solving the problem of low battery capacity and energy density of lithium iron phosphate materials, and achieving Efficient electrochemical performance improvement and production simplification.
Patent Information
- Application Number
- CN202111132340.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-26
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-09-26
AI Technical Summary
The compacted density of lithium iron phosphate material is low, resulting in low specific capacity and energy density of the battery, which limits its application.
By regulating the temperature and time of the lithium iron phosphate material during the sintering process, combining the mixing of spherical and irregular-shaped materials, and using specific sintering and crushing processes, the compacted density of the cathode material is increased.
It achieves high compaction density of lithium iron phosphate cathode material, improves the electrochemical performance and energy density of the battery, simplifies the production process, and saves materials and time.
Smart Images

Figure CN115881945B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of lithium-ion batteries, and in particular to a method for preparing a lithium iron phosphate positive electrode material, a positive electrode sheet and a lithium-ion battery. Background Art
[0002] Lithium iron phosphate materials are widely used in power batteries due to their advantages such as high structural stability, good safety performance, moderate operating voltage and low cost. However, lithium iron phosphate has an obvious disadvantage, which is its low compaction density (usually 2.1-2.3g / cm 3 , seldom can achieve 2.6g / cm 3 The above results in low specific capacity and energy density of the battery made of the material, which hinders the application of the material. Therefore, it is necessary to provide a battery positive electrode material with high compaction density and a preparation method thereof. Summary of the invention
[0003] In view of this, the present application provides a method for preparing a lithium iron phosphate positive electrode material. By regulating the sintering temperature and time of two lithium iron phosphate materials during the preparation process, the high compaction density of the lithium iron phosphate positive electrode material mixed by the two materials can be controlled.
[0004] Specifically, in a first aspect, the present application provides a method for preparing a lithium iron phosphate positive electrode material, comprising the following steps:
[0005] Grinding, spray drying and sintering a first mixed slurry of iron phosphate, lithium source, carbon source and solvent in sequence to obtain a first lithium iron phosphate material with a spherical morphology;
[0006] The second mixed slurry of iron phosphate, lithium source, carbon source and solvent is sequentially ground, spray-dried, sintered and crushed to obtain a second lithium iron phosphate material with irregular morphology;
[0007] The first lithium iron phosphate material and the second lithium iron phosphate material are mixed in equal mass ratios to obtain a lithium iron phosphate positive electrode material; the fitting value C of the maximum compaction density of the lithium iron phosphate positive electrode material satisfies the following relationship:
[0008] C=0.0847t1+0.0196T1-0.0095t2+0.0261T2-33.6716;
[0009] Wherein, T1 and t1 represent the sintering temperature and sintering time of the first lithium iron phosphate material, respectively, T2 and t2 represent the sintering temperature and sintering time of the second lithium iron phosphate material, respectively; t1 and t2 are in the range of 7-11h, T1 is in the range of 760-780°C, T2 is in the range of 770-800°C; and C is 2.6g / cm 3 above.
[0010] The present application controls the sintering temperature and time of two lithium iron phosphate materials with different morphologies during the preparation process, so that the maximum compaction density of the positive electrode material mixed from the two materials can be higher, and the fitting value C of the maximum compaction density of the obtained positive electrode material determined based on the above relationship is very close to the measured value, which can achieve controllable preparation of positive electrode materials with required high compaction density without having to perform compaction density tests on the positive electrode sheets made of the obtained positive electrode materials each time, saving materials and time.
[0011] In this application, the C is 2.6 g / cm 3 At this time, the compaction density of the lithium iron phosphate positive electrode material is significantly higher than the compaction density of the existing lithium iron phosphate positive electrode material (2.1-2.3g / cm 3 In some embodiments of the present application, the C is 2.6-2.85 g / cm 3 In this case, the compaction density of the lithium iron phosphate cathode material is high, and the gram capacity and energy density of the battery made from it are also high.
[0012] In the present application, the preparation of the first lithium iron phosphate material and the second lithium iron phosphate material are similar, and the main difference is that in the process of preparing the second lithium iron phosphate material, after sintering, a crushing process is also performed. The morphology of the first lithium iron phosphate material is spherical, and the morphology of the second lithium iron phosphate material obtained after air flow crushing is irregular. The two types of lithium iron phosphate materials are mixed in a mass ratio of 1:1, so that the second lithium iron phosphate material can be fully filled in the gap between the first lithium iron phosphate material with a large particle size, thereby improving the filling rate and compaction density of the mixture formed by the two. Optionally, the crushing process can be performed in an air flow mill.
[0013] The maximum compaction density A of the first lithium iron phosphate material is less than the maximum compaction density B of the second lithium iron phosphate material. Optionally, A is between 1.8 and 2.2 g / cm 3 The B is in the range of 2.3-2.6 g / cm 3 This is more conducive to obtaining C at 2.6g / cm 3 The above lithium iron phosphate positive electrode material. It should be noted that when the maximum compaction density of a certain material is mentioned in this application, it refers to the maximum compaction density of the positive electrode sheet made of the material.
[0014] In the embodiment of the present application, the D50 particle size of the first lithium iron phosphate material is 3-10 μm. The D50 particle size of the second lithium iron phosphate material is 0.5-3 μm. Generally, the D50 particle size of the first lithium iron phosphate material is larger than the D50 particle size of the second lithium iron phosphate material. This is more conducive to the spherical first lithium iron phosphate material and the irregular second lithium iron phosphate material to form a closer stack.
[0015] In the present application, the composition of the first mixed slurry and the second mixed slurry may be the same or different, wherein the lithium source in the first mixed slurry and the second mixed slurry may be independently selected from one or more of lithium hydroxide (LiOH), lithium carbonate (Li2CO3), lithium oxalate (Li2C2O4), lithium acetate (CH3COOLi), and lithium nitrate (LiNO3), but is not limited thereto. Taking into account that the lithium source has a certain loss during the later sintering process, in the present application, the molar amount of lithium element from the lithium source in the first mixed slurry or the second mixed slurry is controlled to be 1.00-1.05 times the molar amount of the iron phosphate. In other words, the amount of the lithium source and the iron phosphate is such that the molar ratio of lithium element to iron element is (1.00-1.05):1:1.
[0016] The carbon source includes one or more of glucose, starch, phenolic resin, sucrose, cellulose, polyethylene glycol, citric acid, glycine, ethylenediaminetetraacetic acid, agar, acetylene black, Ketjen black, graphite, carbon nanotubes, graphene, etc., but is not limited thereto. Among them, organic carbon sources such as glucose and starch can be decomposed during the sintering process to form a carbon coating layer coated on the surface of the lithium iron phosphate material to give it conductivity; while inorganic carbon sources (such as acetylene black, graphite, etc.) will not decompose during the sintering process, and can also form a carbon coating layer on the surface of the lithium iron phosphate material. An appropriate amount of carbon source can make each lithium iron phosphate material have good conductivity, and can also avoid reducing its charge and discharge specific capacity due to excessive carbon coating, which is ultimately beneficial to the improvement of the electrochemical performance of the lithium iron phosphate positive electrode material. Among them, the amount of carbon source added can ensure that the carbon content in the first lithium iron phosphate material and the second lithium iron phosphate material is 0.5%-3%, preferably 0.8%-2.0%.
[0017] In the present application, the solvent in the first mixed slurry or the second mixed slurry independently includes one or more of water, fatty alcohol (such as methanol, ethanol, propanol, etc.), acetone, N-methylpyrrolidone, etc.
[0018] The grinding described in the present application can be performed in a ball mill, a bead mill or a sand mill, and preferably a grinding device with circulating cooling water. In the process of grinding the first mixed slurry or the second mixed slurry, the grinding power can be 0.5-10 kwh / kg, for example, 1, 2, 5, 8 kwh / kg, etc.
[0019] Optionally, the D50 particle size of the first mixed slurry after grinding is 0.2 μm-5 μm. The D50 particle size of the second mixed slurry after grinding is 0.2 μm-5 μm. This can ensure that the raw materials are fully compounded, and at the same time avoid excessive bond breakage and lattice defects of the raw materials, which affect the electrochemical performance of the prepared lithium iron phosphate material.
[0020] In the embodiment of the present application, when preparing the first lithium iron phosphate material and the second lithium iron phosphate material, the inlet temperature of the spray drying is independently in the range of 150-280°C; and the outlet temperature is independently in the range of 80-120°C.
[0021] The aforementioned T1 and T2 are the sintering and heat preservation temperatures in preparing the first lithium iron phosphate material and the second lithium iron phosphate material. Optionally, during the sintering process, the temperature rise rate to the T1 and T2 can be 2-10°C / min. Appropriate sintering and heat preservation time (i.e., t1, t2) can make the lithium iron phosphate material fully crystallized and have high crystallization integrity. Preferably, the heat preservation time during sintering is 8h-10h.
[0022] The preparation method of the lithium iron phosphate positive electrode material provided in the first aspect of the present application can make the compaction density of the lithium iron phosphate positive electrode material mixed with two lithium iron phosphate materials of different morphologies higher by regulating the sintering temperature and time during the preparation process, and thus the electrochemical performance of the battery prepared by the lithium iron phosphate positive electrode material is better. The preparation method is simple in process, easy to operate, and suitable for large-scale production.
[0023] The second aspect of the present application provides a positive electrode plate, which includes a positive electrode collector and a positive electrode material layer arranged on the surface of the positive electrode collector, and the positive electrode material layer includes a lithium iron phosphate positive electrode material prepared by the above method, a conductive agent and a binder.
[0024] Among them, the maximum compaction density of the positive electrode sheet is substantially consistent with the maximum compaction density C of the positive electrode material calculated according to the formula of the present application. Therefore, without making the positive electrode sheet from the positive electrode material mixed with the first and second lithium iron phosphate materials, the maximum compaction density of the positive electrode sheet made of the positive electrode material can be accurately estimated according to the formula provided in the present application, which can save materials and time.
[0025] A second aspect of the present application provides a lithium-ion battery, which includes a positive electrode plate.
[0026] The lithium-ion battery further includes a negative electrode plate, and an electrolyte and a separator located between the positive electrode plate and the negative electrode plate.
[0027] The lithium-ion battery using the aforementioned positive electrode sheet with high compaction density has a higher discharge specific capacity and a higher energy density. Among them, the button-type lithium-ion battery using the aforementioned positive electrode sheet can have a discharge specific capacity of more than 158 mAh / g at room temperature 0.1C, and in some cases can reach more than 160 mAh / g. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a scanning electron microscope (SEM) photograph of the LFP-1 material used in Example 1.
[0029] Figure 2 This is the SEM photograph of the LFP-2 material used in Example 1. DETAILED DESCRIPTION
[0030] The following are exemplary embodiments of the present invention. It should be noted that a person skilled in the art may make several improvements and modifications without departing from the principles of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present invention.
[0031] The technical solution of the present application is described below in conjunction with a number of specific embodiments.
[0032] Example 1
[0033] A method for preparing a lithium iron phosphate positive electrode material comprises the following steps:
[0034] 1) Preparation of the first lithium iron phosphate material
[0035] a. Weighing iron phosphate, a lithium source (specifically Li2CO3) and a carbon source (specifically glucose monohydrate) at a molar ratio of Li:Fe of 1.03, wherein the amount of the carbon source added can ensure that the carbon content in the first lithium iron phosphate material is 1.5%, dispersing these raw materials in deionized water, mixing them evenly, and preparing a mixed slurry with a solid content of 50%;
[0036] b. Grinding the mixed slurry, the D50 particle size of the ground material is about 0.35 μm, and then spray drying and granulating the ground slurry, wherein the inlet temperature of the spray drying equipment is 200° C. and the outlet temperature is 105° C.;
[0037] c. The granulated powder obtained by spray drying was sintered in a nitrogen atmosphere, wherein the sintering holding temperature T1 during the sintering process was 775° C. and the sintering holding time t1 was 9 h, to obtain the first lithium iron phosphate material LFP-1 with a spherical morphology (SEM photo as shown in FIG. Figure 1 The LFP-1 material was prepared into a positive electrode sheet (refer to the method described below in this embodiment), and its maximum compaction density A was measured to be 2.04 g / cm 3 .
[0038] 2) Preparation of the second lithium iron phosphate material
[0039] The difference between the preparation of LFP-1 and the preparation of LFP-1 is that the sintering holding temperature T2 during the sintering process is 793°C, and the sintering holding time t2 is 8.3h; air flow crushing is also performed after sintering to obtain the second lithium iron phosphate material LFP-2 with irregular morphology (SEM photo as shown in Figure 2The LFP-2 material was prepared into a positive electrode sheet, and its maximum compaction density B was measured to be 2.55 g / cm 3 .
[0040] 3) The above LFP-1 and LFP-2 were mixed in an equal mass ratio to obtain a positive electrode material. According to the above formula C = 0.0847t1 + 0.0196T1 - 0.0095t2 + 0.0261T2 - 33.6716, the fitted value of the maximum compaction density of the positive electrode material was calculated to be C = 2.8991 g / cm 3 .
[0041] The above positive electrode material was prepared into a positive electrode sheet: the positive electrode material was mixed with a binder (specifically polyvinylidene fluoride, PVDF) and conductive carbon black at a mass ratio of 90:5:5, and an appropriate amount of N-methyl ketone pyrrole (NMP) was added thereto. After mixing evenly, a positive electrode slurry was obtained; the positive electrode slurry was coated on one side of a carbon-coated aluminum foil, rolled after drying, and punched into a disc with a diameter of 15 mm to obtain a positive electrode sheet. The actual maximum compaction density of the positive electrode sheet was measured to be 2.88 g / cm 3 , which is basically consistent with the compaction density C of the positive electrode material calculated according to the formula of this application.
[0042] A preparation method for a lithium-ion battery: using a positive electrode sheet made of the above positive electrode material as a positive electrode, a metal lithium sheet as a negative electrode, a polypropylene film as a separator, and a solution of ethylene carbonate (EC) and dimethyl carbonate (DMC) = 1:1 (volume ratio) containing 1.0 mol / L LiPF6 as an electrolyte, and assembling into a button cell in a glove box.
[0043] Example 2
[0044] A method for preparing a lithium iron phosphate positive electrode material, which differs from Example 1 in that:
[0045] The lithium source used is LiOH, and the D50 particle size of the mixed slurry after grinding is about 0.4 μm; when preparing the first lithium iron phosphate material LFP-1, the sintering temperature T1 is 774°C, the sintering holding time t1 is 10h, and the particle size D50 of LFP-1 is measured to be 5.3 μm, and its maximum compaction density A is 2.05 g / cm 3 When preparing the second lithium iron phosphate material LFP-2, the sintering temperature T2 is 788°C, the sintering holding time t2 is 9.8h, the particle size D50 of LFP-2 is measured to be 1.51μm, and its maximum compaction density B is 2.51g / cm 3 .
[0046] According to the above formula C = 0.0847t1 + 0.0196T1 - 0.0095t2 + 0.0261T2 - 33.6716, the fitted value of the maximum compaction density of the positive electrode material obtained in Example 2 is C = 2.8195 g / cm 3 If the positive electrode material is prepared into a positive electrode sheet, its actual maximum compaction density is measured to be 2.81g / cm 3 , which is basically consistent with the calculation result of the formula. According to the same method as in Example 1, the positive electrode sheet of Example 2 is assembled into a button cell.
[0047] Example 3
[0048] A method for preparing a lithium iron phosphate positive electrode material, which differs from Example 1 in that:
[0049] The D50 particle size of the mixed slurry after grinding is about 0.70 μm; when preparing the first lithium iron phosphate material LFP-1, the sintering temperature T1 is 770°C, the sintering holding time t1 is 9h, and the particle size D50 of LFP-1 is measured to be 6.10 μm, and its maximum compaction density A is 2.01 g / cm 3 When preparing the second lithium iron phosphate material LFP-2, the sintering temperature T2 is 795°C, the sintering holding time t2 is 10.4h, the particle size D50 of LFP-2 is measured to be 1.32μm, and its maximum compaction density B is 2.56g / cm 3 .
[0050] According to the above formula C = 0.0847t1 + 0.0196T1 - 0.0095t2 + 0.0261T2 - 33.6716, the fitted value of the maximum compacted density of the positive electrode material obtained in Example 2 is C = 2.8334 g / cm 3 If the positive electrode material is prepared into a positive electrode sheet, its actual maximum compaction density is measured to be 2.82g / cm 3 , which is basically consistent with the calculation result of the formula. According to the same method as in Example 1, the positive electrode sheet of Example 3 is assembled into a button cell.
[0051] Example 4
[0052] A method for preparing a lithium iron phosphate positive electrode material, which differs from Example 1 in that:
[0053] The D50 particle size of the mixed slurry after grinding is about 1.24 μm; when preparing the first lithium iron phosphate material LFP-1, the sintering temperature T1 is 780°C, the sintering holding time t1 is 8.8 h, and the particle size D50 of LFP-1 is measured to be 5.50 μm, and its maximum compaction density A is 2.07 g / cm 3When preparing the second lithium iron phosphate material LFP-2, the sintering temperature T2 is 782°C, the sintering holding time t2 is 10.3h, the particle size D50 of LFP-2 is measured to be 1.02μm, and its maximum compaction density B is 2.45g / cm 3 .
[0054] According to the above formula C = 0.0847t1 + 0.0196T1 - 0.0095t2 + 0.0261T2 - 33.6716, the fitted value of the maximum compaction density of the positive electrode material obtained in Example 2 is C = 2.67411 g / cm 3 If the positive electrode material is prepared into a positive electrode sheet, its actual maximum compaction density is measured to be 2.65g / cm 3 , which is basically consistent with the calculation result of the formula. According to the same method as in Example 1, the positive electrode sheet of Example 4 is assembled into a button cell.
[0055] Example 5
[0056] A method for preparing a lithium iron phosphate positive electrode material, which differs from Example 1 in that:
[0057] The D50 particle size of the mixed slurry after grinding is about 1.12μm; when preparing the first lithium iron phosphate material LFP-1, the sintering temperature T1 is 778℃, the sintering holding time t1 is 10.6h, and the particle size D50 of LFP-1 is measured to be 6.8μm, and its maximum compaction density A is 2.10g / cm 3 When preparing the second lithium iron phosphate material LFP-2, the sintering temperature T2 is 775°C, the sintering holding time t2 is 8.6h, the particle size D50 of LFP-2 is measured to be 1.96μm, and its maximum compaction density B is 2.40g / cm 3 .
[0058] According to the above formula C = 0.0847t1 + 0.0196T1 - 0.0095t2 + 0.0261T2 - 33.6716, the fitted value of the maximum compaction density of the positive electrode material obtained in Example 3 is C = 2.62082 g / cm 3 If the positive electrode material is prepared into a positive electrode sheet, its actual maximum compaction density is measured to be 2.61g / cm 3 , which is basically consistent with the calculation result of the formula. According to the same method as in Example 1, the positive electrode sheet of Example 3 is assembled into a button cell.
[0059] The discharge specific capacity and the first coulombic efficiency of the positive electrode material of the button cell of each embodiment were tested, wherein the button cell was charged and discharged at a constant current of 0.1C within a voltage range of 2.5-3.8V. The results are summarized in Table 1 below.
[0060] Table 1
[0061] Test items Discharge capacity at 0.1C (mAh / g) First effect (%) Example 1 161.5 99.18 Example 2 160.9 99.04 Example 3 161.9 99.14 Example 4 159.4 98.93 Example 5 158.1 98.37
[0062] It can be seen from Table 1 that since the maximum compaction density of the positive electrode sheet made of the positive electrode material of the embodiment of the present application is relatively high, the button battery containing the positive electrode sheet has excellent electrochemical performance and high discharge specific capacity, which is conducive to improving the battery energy density.
[0063] The above only expresses several exemplary embodiments of the present application, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present application. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present application, which all belong to the protection scope of the present application.
Claims
1. A method for preparing a lithium iron phosphate positive electrode material, characterized in that: The following steps are involved: The first mixed slurry of iron phosphate, lithium source, carbon source and solvent is ground, spray dried and sintered in sequence to obtain a first lithium iron phosphate material with a spherical morphology; the maximum compaction density of the first lithium iron phosphate material is 2.01-2.05g / cm 3 within the scope of The second mixed slurry of iron phosphate, lithium source, carbon source and solvent is ground, spray dried, sintered and crushed in sequence to obtain a second lithium iron phosphate material with irregular morphology; the maximum compaction density of the second lithium iron phosphate material is 2.51-2.6g / cm 3 within the scope of The first lithium iron phosphate material and the second lithium iron phosphate material are mixed in equal mass ratios to obtain a lithium iron phosphate positive electrode material; the fitted value of the maximum compaction density of the lithium iron phosphate positive electrode material is recorded as C, and C satisfies the following relationship: C=0.0847t1+0.0196T1-0.0095t2+0.0261T2-33.6716; Wherein, T1 and t1 represent the sintering temperature and sintering time of the first lithium iron phosphate material, respectively, T2 and t2 represent the sintering temperature and sintering time of the second lithium iron phosphate material, respectively; the t1 and t2 are in the range of 7-11h, the T1 is in the range of 760-780°C, the T2 is in the range of 770-800°C; and the C is in the range of 2.8195-2.8991g / cm 3 within the range.
2. The preparation method according to claim 1, characterized in that The particle size D50 of the first lithium iron phosphate material is 3-10 μm.
3. The preparation method according to claim 1, characterized in that: The D50 particle size of the second lithium iron phosphate material is 0.5-3 μm.
4. The preparation method according to claim 1, characterized in that: The D50 particle size of the first mixed slurry or the second mixed slurry after grinding is in the range of 0.2-5 μm.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The molar amount of lithium element in the lithium source is 1.00-1.05 times the molar amount of the iron phosphate.
6. A positive electrode sheet, characterized in that: The positive electrode sheet contains a lithium iron phosphate positive electrode material prepared by the preparation method described in any one of claims 1-5.
7. A lithium ion battery, characterized in that: The lithium-ion battery comprises the positive electrode sheet according to claim 6.
Citation Information
Cited By
Lithium iron phosphate positive electrode material preparation method based on two-step morphology reconstruction
CN122126821A