A bio-based hydroxy polyacrylate emulsion and its preparation method and application
Bio-based hydroxyl polyacrylate emulsions were prepared by reacting bio-based materials and polymer monomers, which solved the problems of environmental pollution and insufficient performance of wood coatings, and realized high-performance waterborne polyurethane coatings that meet environmental protection and performance requirements.
Patent Information
- Application Number
- CN202211623703.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-16
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-12-16
AI Technical Summary
Existing wood coatings pose safety hazards such as environmental pollution and health risks due to organic solvents. Furthermore, the film performance of two-component waterborne polyurethane coatings is not superior to that of petroleum-based materials, making it difficult to meet the requirements for carbon peaking and carbon neutrality.
Bio-based hydroxyl polyacrylate emulsions are prepared using bio-based materials and polymer monomers. Through the condensation reaction of epoxy groups and hydroxyl groups, the water resistance, chemical resistance, and hardness of the coating film are improved, forming a network structure with high cross-linking density.
The prepared bio-based waterborne two-component polyurethane coating has the characteristics of high gloss, high transparency, fast drying, high hardness, excellent chemical resistance, scratch resistance and wear resistance, and meets the requirements of carbon peaking and carbon neutrality.
Smart Images

Figure BDA0004003541090000091 
Figure BDA0004003541090000101 
Figure BDA0004003541090000121
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of coatings, and in particular relates to a bio-based hydroxy polyacrylate emulsion and a preparation method and application thereof. Background Art
[0002] Paint is a substance applied to the surface of an object for the protection, decoration and certain properties of the coated object. Most existing wood coatings are solvent-based coatings, containing more than 50% organic solvents. These solvents will volatilize into the atmosphere during the construction process, polluting the environment and damaging human health. In addition, organic solvents themselves will bring potential safety hazards. Therefore, the water-based nature of wood coatings is the development trend of coatings. Water-based wood coatings include single-component and two-component water-based wood coatings. Among them, the film properties of single-component water-based wood coatings, such as water resistance, chemical resistance and hardness, are quite different from those of oil-based coatings, which seriously limits the promotion and application of water-based wood coatings. The mechanical properties, water resistance and chemical resistance of two-component water-based wood coatings are comparable to those of solvent-based wood coatings, overcoming the shortcomings of single-component water-based wood coatings, and therefore have become the first choice for high-end water-based wood coatings.
[0003] Two-component waterborne polyurethane coatings are composed of waterborne polymer polyols and waterborne polyisocyanate curing agents, which are packaged separately and mixed in proportion when used. Waterborne polymer polyols include waterborne polyacrylate polyols, waterborne polyurethane polyols, waterborne polyester polyols, polyether polyols and mixed polyols. Among them, waterborne polyacrylate polyols have excellent color retention, gloss retention and weather resistance, low price, and easy adjustment of molecular weight, glass transition temperature and hydroxyl content. They are the first choice of waterborne polymer polyols in two-component waterborne polyurethane coatings. Two types of polyacrylate polyols, emulsion and dispersion, can be prepared by different polymerization processes. The hydroxyl content in hydroxy polyacrylate dispersion is relatively high, and the prepared coating film has excellent water resistance and chemical resistance, but it has the disadvantages of complex production process, only 30%-40% solid content of the product, slow drying speed of the paint film, and high cost. Emulsion-type polyacrylate polyols are also called hydroxy polyacrylate emulsions, referred to as hydroxypropylene emulsions, but because of their low hydroxyl content, poor water resistance and chemical resistance of the paint film, their application is limited. In addition, most of the existing two-component water-based polyurethane coatings are petroleum-based materials and do not meet the requirements of carbon peak and carbon neutrality.
[0004] Therefore, there is an urgent need to develop a coating that meets the carbon peak requirements and has a fast drying speed, high hardness and good chemical resistance. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a bio-based hydroxy polyacrylate emulsion, and the paint film of the bio-based waterborne two-component polyurethane coating prepared therefrom has the characteristics of high gloss, high transparency, excellent water resistance and chemical resistance, high crosslinking density, high hardness, scratch resistance and wear resistance.
[0006] The second aspect of the present invention provides a method for preparing the bio-based hydroxy polyacrylate emulsion.
[0007] The third aspect of the present invention provides a coating, wherein the raw materials for preparing the coating include the bio-based hydroxy polyacrylate emulsion.
[0008] A fourth aspect of the present invention provides an application of a coating in the field of decoration.
[0009] According to a first aspect of the present invention, a bio-based hydroxy polyacrylate emulsion is prepared by raw materials including: bio-based materials and polymerized monomers;
[0010] The bio-based material includes a bio-based oil containing an epoxy group;
[0011] The polymerizable monomers include hydroxy acrylate monomers and acrylic acid monomers.
[0012] A bio-based hydroxy polyacrylate emulsion according to an embodiment of the first aspect of the present invention has at least the following beneficial effects:
[0013] The bio-based material reacts with the polymerized monomer to obtain a bio-based hydroxy polyacrylate emulsion. The hydroxyl groups of the bio-based hydroxy polyacrylate emulsion of the present invention are respectively provided directly by the hydroxy acrylate monomer and the epoxy groups of the bio-based material and the carboxyl groups of the polymerized monomer undergo a polycondensation reaction to generate hydroxyl groups, thereby ensuring the water resistance and chemical resistance of the paint film.
[0014] The addition of bio-based materials plays a role in chain extension, increasing the molecular weight of the polymer obtained in the reaction, and can improve the polymer from a linear structure to a network structure. The paint film of the water-based two-component polyurethane coating thus produced has the characteristics of fast drying speed, high hardness and good chemical resistance. In addition, by introducing bio-based materials for reaction, the use of petroleum-based materials is reduced, and it can also meet the country's requirements for carbon peak and carbon neutrality.
[0015] According to some embodiments of the present invention, the epoxy-containing bio-based oil includes at least one of epoxidized soybean oil and epoxidized linseed oil.
[0016] According to some embodiments of the present invention, the epoxidized soybean oil includes at least one of GreenSoft D specialty epoxidized soybean oil and GreenSoft H specialty epoxidized soybean oil.
[0017] According to some embodiments of the present invention, the epoxidized linseed oil comprises epoxidized linseed oil ELO
[0018] According to some embodiments of the present invention, the bio-based content of the bio-based hydroxy polyacrylate emulsion is 5% to 25%.
[0019] According to some embodiments of the present invention, the particle size of the bio-based hydroxy polyacrylate emulsion is 80 nm to 120 nm.
[0020] The particle size within the above range can ensure that the emulsion has a slightly transparent appearance.
[0021] According to some embodiments of the present invention, the solid content of the bio-based hydroxy polyacrylate emulsion is 47-52%.
[0022] According to some embodiments of the present invention, the mass content of hydroxyl groups in the bio-based hydroxy polyacrylate emulsion is 2.5% to 4.6%.
[0023] The hydroxyl content and solid content in the present invention are within the above ranges, which can ensure the versatility of the emulsion in subsequent use and the performance of the paint film.
[0024] According to some embodiments of the present invention, the raw materials for preparing the polyacrylate polymer containing hydroxyl groups further include acrylate monomers and vinyl monomers.
[0025] According to some embodiments of the present invention, in parts by weight, the acrylic monomer is 4 to 7 parts, the acrylate monomer is 15 to 35 parts, the vinyl monomer is 5 to 10 parts, the hydroxy acrylate monomer is 5 to 15 parts and the bio-based material is 9 to 15 parts.
[0026] According to some embodiments of the present invention, the acrylic monomer includes at least one of an acrylic monomer and a methacrylic monomer.
[0027] According to some embodiments of the present invention, the acrylate monomer includes at least one of methyl methacrylate, butyl acrylate, isobornyl acrylate, cyclohexyl methacrylate and benzyl methacrylate.
[0028] According to some embodiments of the invention, the vinyl monomer comprises styrene.
[0029] According to some embodiments of the present invention, the hydroxyacrylate monomer includes at least one of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate and hydroxypropyl methacrylate.
[0030] According to an embodiment of the second aspect of the present invention, a method for preparing a bio-based hydroxy polyacrylate emulsion is provided, comprising a mixing reaction of the bio-based material and the polymerization monomer.
[0031] According to some embodiments of the present invention, in the mixing reaction of the bio-based material and the polyacrylate polymer containing hydroxyl groups, the reaction temperature is 150-170°C.
[0032] According to some embodiments of the present invention, in the mixing reaction of the bio-based material and the polyacrylate polymer containing hydroxyl groups, the reaction pressure is 1.9-2.5 MPa.
[0033] According to some embodiments of the present invention, in the mixing reaction of the bio-based material and the polyacrylate polymer containing hydroxyl groups, the mixing reaction time is 45 to 80 minutes.
[0034] According to some embodiments of the present invention, the raw materials for preparing the polyacrylate polymer include: polyacrylate polymer, emulsifier, deionizer and neutralizer 1.
[0035] According to some preferred embodiments of the present invention, the method for preparing the polyacrylate polymer comprises:
[0036] S1: uniformly mixing the acrylic acid monomer, the acrylic ester monomer, the vinyl monomer, the hydroxy acrylic ester monomer and the bio-based material to form a mixed solution A for standby use;
[0037] S2: Mix deionized water, emulsifier and monomer mixed solution A to obtain pre-emulsion solution B for standby use;
[0038] S3: mixing ionized water, initiator and emulsifier to obtain a mixed solution C for standby use;
[0039] S4: Mix deionized water and neutralizer 1 to form a mixed solution D for later use;
[0040] S5: After deionized water, an emulsifier and a buffer are mixed, stirred and heated, a portion of the pre-emulsion B is added to obtain a seed emulsion, and then the remaining pre-emulsion B and mixed solutions C and D are added to react to obtain a bio-based hydroxy polyacrylate emulsion.
[0041] According to some embodiments of the present invention, the mixed liquid A in step S1 includes, by weight, 4 to 7 parts of acrylic acid monomers, 15 to 35 parts of acrylate monomers, 5 to 10 parts of vinyl monomers, 5 to 15 parts of hydroxy acrylate monomers and 9 to 15 parts of bio-based materials.
[0042] According to some embodiments of the present invention, the pre-emulsion B in step S2 includes, by weight, 28 to 33 parts of deionized water, 0.45 to 2.1 parts of emulsifier, and 55.75 to 60.8 parts of monomer mixed solution A.
[0043] According to some preferred embodiments of the present invention, step S2 includes dissolving 0.45 to 2.1 parts of emulsifier in 28 to 33 parts of deionized water, stirring evenly, adjusting the disperser to 700 rpm, dripping 55.75 to 60.8 parts of monomer mixed solution A, dripping for 15 to 25 minutes, and continuing to disperse for 10 to 20 minutes after dripping to obtain pre-emulsion B for standby use.
[0044] According to some embodiments of the present invention, the mixed solution C in step S3 includes, by weight, 5 to 7 parts of deionized water, 0.2 to 0.6 parts of initiator, and 0 to 1 parts of emulsifier.
[0045] According to some embodiments of the present invention, the mixed solution D in step S4 includes 5 to 8.5 parts of deionized water and 0.5 to 0.7 parts of neutralizer 1 by weight.
[0046] According to some embodiments of the present invention, the bio-based hydroxy polyacrylate emulsion in step S5 includes, by weight, 19 to 25 parts of deionized water, 0.3 to 0.8 parts of emulsifier, 0.1 to 0.5 parts of buffer, 83 to 96 parts of pre-emulsion B, 5.5 to 8.5 parts of mixed solution C and 5.5 to 9.5 parts of mixed solution D.
[0047] According to some embodiments of the invention, the initiator comprises a persulfate.
[0048] According to some embodiments of the present invention, the emulsifier includes at least one of a non-reactive emulsifier and a reactive emulsifier.
[0049] According to some embodiments of the present invention, the non-reactive emulsifier includes at least one of sodium dodecyl sulfate (SDS), Dow's isomeric alcohol polyoxyethylene ether (EH-9), DOWFAX-2A1 and fatty alcohol polyoxyethylene ether ammonium sulfate (KL-525).
[0050] According to some embodiments of the present invention, the reactive emulsifier includes at least one of sodium 3-allyloxy-1-hydroxypropane sulfonate (COPS-1), sodium 2-acrylamido-2-methylpropane sulfonate (COPS-2), SR-10 and ER-30.
[0051] According to some embodiments of the present invention, the neutralizer 1 includes a neutralizer containing a tertiary amine.
[0052] According to some embodiments of the present invention, the neutralizing agent 1 includes at least one of triethylamine (TEA), N,N-dimethylethanolamine (DMEA) and N,N-dimethylcyclohexylamine (DMCHA).
[0053] According to some embodiments of the present invention, the buffer comprises at least one of sodium bicarbonate (NaHCO 3 ) and sodium carbonate (Na 2 CO 3 ).
[0054] According to some embodiments of the present invention, the initiator includes at least one of potassium persulfate (KPS) and ammonium persulfate (APS).
[0055] According to an embodiment of the third aspect of the present invention, a coating is provided, wherein the raw materials for preparing the coating include the bio-based hydroxy polyacrylate emulsion.
[0056] According to some embodiments of the present invention, the coating preparation method includes mixing agent A and agent B at an NCO / OH molar ratio of 1.0-1.8:1 during construction;
[0057] In parts by weight, the agent A comprises: 60-65 parts of bio-based hydroxy polyacrylate emulsion, 30-36 parts of water, 2-4 parts of film-forming aid, 0.05-0.2 parts of defoaming agent, 0.5-0.8 parts of thickener, 0.05-0.2 parts of wetting agent and 0.2-0.5 parts of neutralizer 2;
[0058] In parts by weight, the agent B comprises: 15-30 parts of water-based polyisocyanate curing agent.
[0059] In the present invention, the NCO / OH molar ratio is 1.0-1.8:1. Under this ratio, the low hardness and poor resistance of the paint film caused by a too low ratio and the appearance of "prickly heat" and other defects on the paint film surface caused by a too high ratio are avoided.
[0060] According to some embodiments of the present invention, the film-forming aid includes at least one of propylene glycol methyl ether, propylene glycol butyl ether, dipropylene glycol methyl ether and dipropylene glycol butyl ether.
[0061] According to some embodiments of the present invention, the defoaming agent includes at least one of a polyether siloxane copolymer defoaming agent and a modified polysiloxane copolymer solution.
[0062] According to some embodiments of the present invention, the polyether siloxane copolymer defoamer includes at least one of TEGO-800, TEGO-805, TEGO-815 and TEGO-825.
[0063] According to some embodiments of the present invention, the modified polysiloxane copolymer solution includes at least one of BYK-019 and BYK-020.
[0064] According to some embodiments of the present invention, the thickener includes at least one of a nonionic polyurethane associative thickener, a hydrophobically modified alkali-swellable associative thickener, an alkali-swellable non-associative thickener, and a nonionic associative thickener.
[0065] According to some embodiments of the present invention, the nonionic polyurethane associative thickener includes RM-8W.
[0066] According to some embodiments of the present invention, the hydrophobically modified alkali-swellable associative thickener is TT-935.
[0067] According to some embodiments of the present invention, the alkali-swellable non-associative thickener includes ASE-60.
[0068] According to some embodiments of the present invention, the nonionic associative thickener includes at least one of TEGO ViscoPlus 3000, TEGO ViscoPlus 3030, and TEGO ViscoPlus 3060.
[0069] According to some embodiments of the present invention, the wetting agent includes at least one of a polyether siloxane copolymer, a nonionic organic surfactant, and a polyether-modified polysiloxane solution.
[0070] According to some embodiments of the present invention, the polyether siloxane copolymer includes TEGO-245.
[0071] According to some embodiments of the present invention, the nonionic organic surfactant includes TEGO-500.
[0072] According to some embodiments of the present invention, the polyether-modified polysiloxane solution includes BYK-346.
[0073] According to some embodiments of the present invention, the neutralizer 2 includes at least one of triethylamine and dimethylethanolamine.
[0074] According to some embodiments of the present invention, the polyisocyanate curing agent includes at least one of sulfonates, carboxylates, and alkoxy hydrophilically modified hexamethylene diisocyanate (HDI).
[0075] According to some embodiments of the present invention, the polyisocyanate curing agent includes at least one of Bayhydur XP2487 / 1 and Bayhydur XP 2655.
[0076] According to some embodiments of the present invention, the method for preparing the bio-based waterborne two-component polyurethane coating comprises the following steps:
[0077] Premix water and film-forming aids and add them to hydroxy polyacrylate emulsion, then add defoamer, thickener, wetting agent and neutralizer 2 in sequence, disperse for 10-30 minutes, and filter to obtain agent A;
[0078] During construction, the water-based polyisocyanate curing agent is added to the A agent according to the NCO / OH molar ratio of 1.0-1.8, and stirred for 5-8 minutes to obtain a bio-based water-based two-component polyurethane coating.
[0079] The present invention uses the bio-based two-component polyurethane coating agent A and agent B prepared by the above method in combination, and the obtained bio-based water-based two-component polyurethane coating film has the advantages of high gloss, high transparency, excellent water resistance and chemical resistance, high cross-linking density, high hardness, scratch resistance, wear resistance and fast drying speed, and can be applied to high-end wood coatings, automotive coatings, metal anti-corrosion coatings and other industrial protective coatings.
[0080] According to an embodiment of the fourth aspect of the present invention, a coating is used in the field of decoration.
[0081] According to some embodiments of the present invention, the coating decoration field includes wood products.
[0082] According to some embodiments of the present invention, the coating decoration field includes metal.
[0083] According to some embodiments of the present invention, the paint decoration field includes automobiles.
[0084] According to some embodiments of the present invention, the coating decoration field includes metal corrosion protection. DETAILED DESCRIPTION
[0085] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0086] The (meth)acrylic acid monomer is acrylic acid or methacrylic acid from Miki Corporation;
[0087] The (meth)acrylate monomers are methyl methacrylate, butyl acrylate, isobornyl acrylate, cyclohexyl methacrylate, and benzyl methacrylate from Sanmu Company;
[0088] The vinyl monomer was styrene from Miki Corporation;
[0089] The hydroxy acrylate monomer is hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate or hydroxypropyl methacrylate of Changxing Company;
[0090] The non-reactive emulsifiers are sodium dodecyl sulfate (SDS) from BASF, isomeric alcohol polyoxyethylene ether (EH-9) and DOWFAX-2A1 from Dow, and fatty alcohol polyoxyethylene ether ammonium sulfate (KL-525) from Guangzhou Hangqin.
[0091] The reactive emulsifiers were 3-allyloxy-1-hydroxypropane sulfonate (COPS-1) and 2-acrylamido-2-methylpropane sulfonate (COPS-2) from Solvay, and SR-10 and ER-30 from Japan Aidico;
[0092] The buffers are sodium bicarbonate (NaHCO3) and sodium carbonate (Na2CO3) from Xilong Chemical;
[0093] The initiators are potassium persulfate (KPS) and ammonium persulfate (APS) from Xilong Chemical;
[0094] The bio-based materials are GreenSoft D special epoxy soybean oil, GreenSoft H special epoxy soybean oil, and epoxy linseed oil from Xingbang Polymer Materials Co., Ltd.
[0095] The defoamers are TEGO's polyether siloxane copolymer defoamers TEGO-800, TEGO-805, TEGO-815, TEGO-825, BYK's modified polysiloxane copolymer solutions BYK-019 and BYK-020;
[0096] The thickeners are DOW's nonionic polyurethane associative thickener RM-8W, hydrophobically modified alkali-swellable associative thickener TT-935, alkali-swellable non-associative thickener ASE-60, TEGO's nonionic associative thickeners TEGOViscoPlus 3000, TEGO ViscoPlus 3030, TEGO ViscoPlus 3060; the wetting agents are TEGO's polyether siloxane copolymer TEGO-245, nonionic organic surfactant TEGO-500, BYK's polyether-modified polysiloxane solution BYK-346;
[0097] The neutralizing agents were triethylamine and dimethylethanolamine from Dow;
[0098] Polyisocyanate curing agents include sulfonates, carboxylates, and alkoxy hydrophilically modified hexamethylene diisocyanate (HDI);
[0099] The polyisocyanate curing agents were Bayhydur XP 2487 / 1 and Bayhydur XP 2655 from Covestro;
[0100] Example 1
[0101] A bio-based hydroxy polyacrylate emulsion 1 is prepared by the following steps:
[0102] S1. In parts by mass, 5.7 parts of acrylic acid, 5.5 parts of cyclohexyl methacrylate, 10 parts of methyl methacrylate, 5 parts of butyl acrylate, 7 parts of styrene, 10 parts of hydroxyethyl methacrylate, and 15 parts of epoxy soybean oil GreenSoft H were mixed to form a mixed solution A1 for standby use;
[0103] S2. Add 33 parts of deionized water to the dispersion tank, dissolve 0.5 parts of SDS and 1 part of EH-9, stir well and adjust the disperser to 700 rpm, add 58.2 parts of the mixture A1, drip it for 25 minutes, continue to disperse for 10 minutes after dripping, and obtain the pre-emulsion B1 for standby;
[0104] S3. Dissolve 0.45 parts of APS and 1 part of COPS-1 in 7 parts of deionized water to form a mixed solution C1 for standby use;
[0105] S4. By mass, 8.5 parts of deionized water and 0.6 parts of DMEA were mixed to form a mixed solution D1 for standby use;
[0106] S5. Add 19.95 parts of deionized water, 0.25 parts of SDS, 0.5 parts of EH-9, 0.2 parts of Na2CO3 and 0.15 parts of APS to a four-necked flask equipped with a thermometer, a condenser, a stirring paddle and a constant pressure dropping funnel, mix and stir and heat. When the temperature reaches 77°C, add 9.3 parts of pre-emulsion B1 dropwise over 15 minutes, and stabilize for 10 minutes after the dropwise addition to obtain a seed emulsion. Raise the temperature to 80°C, and simultaneously add 83.4 parts of pre-emulsion B1 and 8.45 parts of mixed solution C1 dropwise over 3.5 hours, and then raise the temperature to 85°C after the dropwise addition, keep the temperature for 2 hours, cool down to 55°C, add 9.1 parts of mixed solution D1, stir for 10 minutes, and transfer to a high-pressure reactor, pressurize to 2MPa, heat to 160°C, react for 60 minutes, and stop the reaction after the epoxy value is less than 0.005 as determined by the hydrochloric acid-acetone method.
[0107] S6. Cool down to 40° C., release the pressure, and filter the material to obtain the bio-based hydroxy polyacrylate emulsion 1.
[0108] Example 2
[0109] Example A bio-based waterborne two-component polyurethane coating 1 was prepared. The bio-based hydroxy polyacrylate emulsion was prepared in Example 1. The specific steps were:
[0110] During construction, mix A1 and B1 agents at a NCO / OH molar ratio of 1.8:1;
[0111] Wherein, agent A1 is composed of the following components in parts by weight:
[0112]
[0113] Agent B1 is a water-based polyisocyanate curing agent, the water-based polyisocyanate curing agent is Bayhydur XP2487 / 1, and the mass fraction of Bayhydur XP 2487 / 1 is 24.9 parts;
[0114] The preparation method of agent A1 is as follows: add bio-based hydroxy polyacrylate emulsion 1 into a stirring tank at a rotation speed of 700 rpm, premix water, dipropylene glycol butyl ether and dipropylene glycol methyl ether and add them into the stirring tank, add TEGO-800, RM-8W, TEGO-245 and TEA in sequence, disperse for 20 minutes, and filter the material.
[0115] During construction, agent B1 was added to agent A1 and stirred for 6 minutes to obtain a bio-based waterborne two-component polyurethane coating 1, whose bio-based content was 12.2%.
[0116] The paint film prepared from the bio-based waterborne two-component polyurethane coating 1 was cured and dried at room temperature for 7 days, and its properties are shown in Table 1.
[0117] Example 3
[0118] A bio-based hydroxy polyacrylate emulsion 2 is prepared by the following steps:
[0119] S1. By mass, 4.3 parts of methacrylic acid, 10 parts of isobornyl acrylate, 11 parts of methyl methacrylate, 10.45 parts of butyl acrylate, 5.5 parts of styrene, 5.5 parts of hydroxyethyl acrylate, and 9 parts of epoxy soybean oil GreenSoft D were mixed to form a mixed solution A2 for standby use;
[0120] S2. Add 28 parts of deionized water to the dispersion tank, dissolve 0.45 parts of KL-525, stir well and adjust the disperser to 700 rpm, add 55.75 parts of the mixture A2, drip for 20 minutes, continue to disperse for 8 minutes after dripping, and obtain the pre-emulsion B2 for standby;
[0121] S3. In parts by mass, 0.2 parts of KPS and 0.75 parts of COPS-2 were dissolved in 5 parts of deionized water to form a mixed solution C2 for standby use;
[0122] S4. In parts by mass, 5.5 parts of deionized water and 0.5 parts of TEA were mixed to form a mixed solution D2 for standby use;
[0123] S5. Add 20 parts of deionized water, 0.3 parts of KL-525, 0.15 parts of NaHCO3 and 0.1 parts of KPS to a four-necked flask equipped with a thermometer, a condenser, a stirring paddle and a constant pressure dropping funnel, mix and stir and heat. When the temperature reaches 80°C, add 6.7 parts of pre-emulsion B2 in 20 minutes, stabilize for 15 minutes after the drop is complete to obtain a seed emulsion. The temperature is maintained at 80°C, and 77.5 parts of pre-emulsion B2 and 5.95 parts of mixed solution C2 are added at the same time. The drop is completed in 4 hours. After the drop is completed, the temperature is raised to 90°C, kept warm for 1 hour, cooled to 50°C, 6 parts of mixed solution D2 are added, stirred for 8 minutes, and then transferred to a high-pressure reactor, pressurized to 1.9MPa, heated to 150°C, reacted for 80 minutes, and the reaction was stopped after the epoxy value was less than 0.005 measured by the hydrochloric acid-acetone method.
[0124] S6. Cool down to 40°C, release the pressure, and filter the material to obtain the bio-based hydroxy polyacrylate emulsion 2.
[0125] Example 4
[0126] This example also prepares a bio-based water-based two-component polyurethane coating 2, and the bio-based hydroxy polyacrylate emulsion is prepared in Example 3, and the specific steps are as follows:
[0127] During construction, mix A2 and B2 agents at a NCO / OH molar ratio of 1.8:1;
[0128] Wherein, agent A2 is composed of the following components in parts by weight:
[0129]
[0130]
[0131] Agent B2 is a water-based polyisocyanate curing agent, the water-based polyisocyanate curing agent is Bayhydur XP 2655, and the mass fraction of Bayhydur XP 2655 is 17.4 parts;
[0132] The preparation method of the A2 agent of the above-mentioned bio-based water-based two-component polyurethane coating 2 is as follows: add the bio-based hydroxy polyacrylate emulsion 2 into a stirring tank at a rotation speed of 700 rpm, premix water, dipropylene glycol butyl ether and dipropylene glycol methyl ether and add them into the stirring tank, add TEGO-805, TT-935, BYK-346 and DMEA in sequence, disperse for 10 minutes, and filter the material.
[0133] During construction, agent B2 was added to agent A2 and stirred for 5 minutes to obtain a bio-based waterborne two-component polyurethane coating 2, whose bio-based content was 9.4%.
[0134] The paint film prepared from the bio-based waterborne two-component polyurethane coating 2 was cured and dried at room temperature for 7 days, and its properties are shown in Table 1.
[0135] Example 5
[0136] A bio-based hydroxy polyacrylate emulsion 3 is prepared by the following steps:
[0137] S1. By mass, 6.3 parts of acrylic acid, 5 parts of benzyl methacrylate, 5 parts of methyl methacrylate, 7 parts of butyl acrylate, 10 parts of styrene, 15 parts of hydroxypropyl methacrylate, 12.5 parts of epoxy linseed oil were added. Mix well to form mixed solution A3 for later use;
[0138] S2. Add 30 parts of deionized water to the dispersion tank, dissolve 0.6 parts of DOWFAX-2A1, 0.5 parts of SR-10, and 1 part of ER-30, stir well, adjust the disperser to 700 rpm, add 60.8 parts of the mixture A3, drip for 30 minutes, continue to disperse for 12 minutes after dripping, and obtain a pre-emulsion B3 standby;
[0139] S3. In parts by mass, 0.6 parts of APS were dissolved in 6 parts of deionized water to form a mixed solution C3 for standby use;
[0140] S4. In parts by mass, 5 parts of deionized water and 0.7 parts of DMCHA were mixed to form a mixed solution D3 for standby use;
[0141] S5. Add 24.5 parts of deionized water, 0.5 parts of DOWFAX-2A1, 0.2 parts of SR-10, 0.5 parts of NaHCO3 and 0.1 parts of KPS to a four-necked flask equipped with a thermometer, a condenser, a stirring paddle and a constant pressure dropping funnel, mix and heat, and when the temperature reaches 83°C, drip 11 parts of pre-emulsion B3 in 25 minutes, and stabilize for 20 minutes after dripping to obtain a seed emulsion. Raise the temperature to 85°C, and simultaneously drip 81.9 parts of pre-emulsion B3 and 6.6 parts of mixed solution C3, drip them in 5 hours, maintain 85°C after dripping, keep warm for 1.5 hours, cool to 60°C, add 7.5 parts of mixed solution D3, stir for 12 minutes, transfer to a high-pressure reactor, pressurize to 2.5MPa, heat to 170°C, react for 45 minutes, and stop the reaction when the epoxy value is less than 0.005 determined by the hydrochloric acid-acetone method;
[0142] S6. Cool down to 40° C., release the pressure, and filter the material to obtain the bio-based hydroxy polyacrylate emulsion 3.
[0143] Example 6
[0144] A bio-based waterborne two-component polyurethane coating 3 was prepared in the embodiment. The bio-based hydroxy polyacrylate emulsion was prepared in the embodiment 5. The specific steps are as follows:
[0145] During construction, mix A3 and B3 agents at a NCO / OH molar ratio of 1.8:1;
[0146] Wherein, the A3 agent comprises the following components in parts by weight:
[0147]
[0148] Agent B3 is a water-based polyisocyanate curing agent, the water-based polyisocyanate curing agent is Bayhydur XP2487 / 1, and the mass fraction of Bayhydur XP 2487 / 1 is 29.9 parts;
[0149] The preparation method of the A3 agent of the above-mentioned bio-based water-based two-component polyurethane coating 3 is as follows: add the bio-based hydroxy polyacrylate emulsion 3 into a stirring tank at a rotation speed of 700 rpm, premix water, dipropylene glycol butyl ether and dipropylene glycol methyl ether and add them into the stirring tank, add TEGO-805, TT-935, BYK-346 and DMEA in sequence, disperse for 30 minutes, and filter the material.
[0150] During construction, agent B3 was added to agent A3 and stirred for 8 minutes to obtain a bio-based waterborne two-component polyurethane coating 3, whose bio-based content was 8.9%.
[0151] The paint film prepared from the bio-based waterborne two-component polyurethane coating 3 was cured and dried at room temperature for 7 days, and its properties are shown in Table 1.
[0152] Comparative Example 1
[0153] The difference between this comparative example and Example 1 is that the hydroxy polyacrylate emulsion synthesized from bio-based materials is not added, and the specific steps are as follows:
[0154] S1. In parts by mass, 5.7 parts of acrylic acid, 5.5 parts of cyclohexyl methacrylate, 10 parts of methyl methacrylate, 5 parts of butyl acrylate, 7 parts of styrene, and 10 parts of hydroxyethyl methacrylate were mixed to form a mixed solution A4 for standby use;
[0155] S2. Add 33 parts of deionized water to the dispersion tank, dissolve 0.5 parts of SDS and 1 part of EH-9, stir well and adjust the disperser to 700 rpm, add 43.2 parts of the mixture A4, drip it for 25 minutes, continue to disperse for 10 minutes after dripping, and obtain the pre-emulsion B4 standby;
[0156] S3. In parts by mass, 0.45 parts of APS and 1 part of COPS-1 were dissolved in 7 parts of deionized water to form a mixed solution C4 for standby use;
[0157] S4. By mass, 8.5 parts of deionized water and 0.6 parts of DMEA were mixed to form a mixed solution D4 for standby use;
[0158] S5. Add 19.95 parts of deionized water, 0.25 parts of SDS, 0.5 parts of EH-9, 0.2 parts of Na2CO3 and 0.15 parts of APS to a four-necked flask equipped with a thermometer, a condenser, a stirring paddle and a constant pressure dropping funnel, mix and heat, and when the temperature reaches 77°C, add 7.8 parts of pre-emulsion B4 dropwise over 15 minutes, and stabilize for 10 minutes after the addition to obtain a seed emulsion. Raise the temperature to 80°C, and simultaneously add 69.9 parts of pre-emulsion B4 and 8.45 parts of mixed solution C4 dropwise over 3.5 hours, and then raise the temperature to 85°C after the addition, keep warm for 2 hours, cool to 55°C, add 9.1 parts of mixed solution D4, stir for 10 minutes, and transfer to a high-pressure reactor, pressurize to 2MPa, heat to 160°C, react for 60 minutes, and stop the reaction when the epoxy value is less than 0.005 as determined by the hydrochloric acid-acetone method;
[0159] S6. Cool down to 40°C, filter the material to obtain hydroxy polyacrylate emulsion 4.
[0160] Comparative Example 2
[0161] Comparative Example A water-based two-component polyurethane coating 4 was prepared, and the emulsion was prepared in Comparative Example 1. The specific steps were:
[0162] During construction, mix A4 and B4 agents at a NCO / OH molar ratio of 1.8:1;
[0163] Wherein, the A4 agent comprises the following components in parts by weight:
[0164]
[0165] Agent B4 is a water-based polyisocyanate curing agent, the water-based polyisocyanate curing agent is Bayhydur XP2487 / 1, and the mass fraction of Bayhydur XP 2487 / 1 is 15.3 parts;
[0166] The preparation method of the A4 agent of the above-mentioned water-based two-component polyurethane coating 4 is as follows: add the hydroxy polyacrylate emulsion 4 into a stirring tank at a rotation speed of 700 rpm, premix water, dipropylene glycol butyl ether and dipropylene glycol methyl ether and add them into the stirring tank, add TEGO-800, RM-8W, TEGO-245 and TEA in sequence, disperse for 20 minutes, and filter the material.
[0167] During construction, agent B4 was added to agent A4 and stirred for 6 minutes to obtain a water-based two-component polyurethane coating 4, whose biobased content was 0%.
[0168] The paint film prepared by the water-based two-component polyurethane coating 4 was cured and dried at room temperature for 7 days, and its properties are shown in Table 1.
[0169] Comparative Example 3
[0170] This comparative example is a hydroxy polyacrylate emulsion synthesized by conventional process without adding bio-based materials. The specific steps are:
[0171] S1. In parts by mass, 0.9 parts of acrylic acid, 5.5 parts of cyclohexyl methacrylate, 10 parts of methyl methacrylate, 16.1 parts of butyl acrylate, 7 parts of styrene, and 18.7 parts of hydroxyethyl methacrylate were mixed to form a mixed solution A5 for standby use;
[0172] S2. Add 33 parts of deionized water to the dispersion tank, dissolve 0.5 parts of SDS and 1 part of EH-9, stir well and adjust the disperser to 700 rpm, add 58.2 parts of the mixture A5, drip it for 25 minutes, continue to disperse for 10 minutes after dripping, and obtain the pre-emulsion B5 standby;
[0173] S3. In parts by mass, 0.45 parts of APS and 1 part of COPS-1 were dissolved in 7 parts of deionized water to form a mixed solution C5 for standby use;
[0174] S4. By mass, 8.5 parts of deionized water and 0.6 parts of DMEA were mixed to form a mixed solution D5 for standby use;
[0175] S5. Add 19.95 parts of deionized water, 0.25 parts of SDS, 0.5 parts of EH-9, 0.2 parts of NaHCO3 and 0.15 parts of APS to a four-necked flask equipped with a thermometer, a condenser, a stirring paddle and a constant pressure dropping funnel, mix and heat, and when the temperature reaches 77°C, add 9.3 parts of pre-emulsion B5 dropwise over 15 minutes, and stabilize for 10 minutes after the addition to obtain a seed emulsion. Raise the temperature to 80°C, and simultaneously add 83.4 parts of pre-emulsion B5 and 8.45 parts of mixed solution C5 dropwise, and add dropwise over 3.5 hours. After the addition, raise the temperature to 85°C, keep warm for 2 hours, cool to 55°C, add 9.1 parts of mixed solution D5, stir for 10 minutes, and transfer to a high-pressure reactor, pressurize to 2MPa, heat to 160°C, react for 60 minutes, and stop the reaction when the epoxy value is less than 0.005 as determined by the hydrochloric acid-acetone method;
[0176] S6. Cool down to 40°C, release the pressure, and filter the material to obtain hydroxy polyacrylate emulsion 5.
[0177] Comparative Example 4
[0178] A water-based two-component polyurethane coating 5 was prepared in the comparative example. The emulsion was prepared in the comparative example 3. The specific steps were as follows:
[0179] During construction, mix A5 and B5 agents at a NCO / OH molar ratio of 1.8:1;
[0180] Wherein, the A5 agent comprises the following components in parts by weight:
[0181]
[0182] Agent B5 is a water-based polyisocyanate curing agent, the water-based polyisocyanate curing agent is Bayhydur XP2487 / 1, and the mass fraction of Bayhydur XP 2487 / 1 is 24.9 parts;
[0183] The preparation method of the A5 agent of the above-mentioned bio-based water-based two-component polyurethane coating 5 is as follows: add the hydroxy polyacrylate emulsion 5 into a stirring tank at a rotation speed of 700 rpm, premix water, dipropylene glycol butyl ether and dipropylene glycol methyl ether and add them into the stirring tank, add TEGO-800, RM-8W, TEGO-245 and TEA in sequence, disperse for 20 minutes, and filter the material.
[0184] During construction, agent B5 was added to agent A5 and stirred for 6 minutes to obtain a water-based two-component polyurethane coating 5, whose bio-based content was 0%.
[0185] The paint film prepared from the bio-based waterborne two-component polyurethane coating 5 was cured and dried at room temperature for 7 days, and its properties are shown in Table 1.
[0186] Comparative Example 5
[0187] This comparative example is to synthesize the bio-based hydroxy polyacrylate emulsion without adding hydroxy acrylate monomer. The specific steps are:
[0188] S1. By mass, 11.2 parts of acrylic acid, 2.9 parts of cyclohexyl methacrylate, 5.3 parts of methyl methacrylate, 2.7 parts of butyl acrylate, 3.4 parts of styrene, and 32.3 parts of epoxy soybean oil GreenSoft H were mixed to form a mixed solution A6 for standby use;
[0189] S2. Add 33 parts of deionized water to the dispersion tank, dissolve 0.5 parts of SDS and 1 part of EH-9, stir well and adjust the disperser to 700 rpm, add 58.2 parts of the mixture A6, drip it for 25 minutes, continue to disperse for 10 minutes after dripping, and obtain the pre-emulsion B6 standby;
[0190] S3. In parts by mass, 0.45 parts of APS and 1 part of COPS-1 were dissolved in 7 parts of deionized water to form a mixed solution C6 for standby use;
[0191] S4. In parts by mass, 8.5 parts of deionized water and 0.6 parts of DMEA were mixed to form a mixed solution D6 for standby use;
[0192] S5. Add 19.95 parts of deionized water, 0.25 parts of SDS, 0.5 parts of EH-9, 1 part of Na2CO3 and 0.15 parts of APS to a four-necked flask equipped with a thermometer, a condenser, a stirring paddle and a constant pressure dropping funnel, mix and heat, and when the temperature reaches 77°C, add 9.3 parts of pre-emulsion B6 dropwise over 15 minutes, and stabilize for 10 minutes after the addition to obtain a seed emulsion. Raise the temperature to 80°C, and simultaneously add 83.4 parts of pre-emulsion B6 and 8.45 parts of mixed solution C6 dropwise over 3.5 hours, and then raise the temperature to 85°C after the addition, keep warm for 2 hours, cool to 55°C, add 9.1 parts of mixed solution D6, stir for 10 minutes, and transfer to a high-pressure reactor, pressurize to 2MPa, heat to 160°C, react for 60 minutes, and stop the reaction when the epoxy value is less than 0.005 as determined by the hydrochloric acid-acetone method;
[0193] S6. Cool down to 40°C, release the pressure, and filter the material to obtain hydroxy polyacrylate emulsion 6.
[0194] Comparative Example 6
[0195] A water-based two-component polyurethane coating 6 was prepared in the comparative example. The emulsion was prepared in the comparative example 5. The specific steps were as follows:
[0196] During construction, mix A6 and B6 agents at a NCO / OH molar ratio of 1.8:1;
[0197] Wherein, the A6 agent comprises the following components in parts by weight:
[0198]
[0199] Agent B6 is a water-based polyisocyanate curing agent, the water-based polyisocyanate curing agent is Bayhydur XP2487 / 1, and the mass fraction of Bayhydur XP 2487 / 1 is 24.9 parts;
[0200] The preparation method of the A6 agent of the above-mentioned water-based two-component polyurethane coating 6 is as follows: add the hydroxy polyacrylate emulsion 6 into a stirring tank at a rotation speed of 700 rpm, premix water, dipropylene glycol butyl ether and dipropylene glycol methyl ether and add them into the stirring tank, add TEGO-800, RM-8W, TEGO-245 and TEA in sequence, disperse for 20 minutes, and filter the material.
[0201] During construction, agent B6 was added to agent A6 and stirred for 6 minutes to obtain a water-based two-component polyurethane coating 6, whose biobased content was 26.4%.
[0202] The paint film prepared from the bio-based waterborne two-component polyurethane coating 6 was cured and dried at room temperature for 7 days, and its properties are shown in Table 1.
[0203] Comparative Example 7
[0204] This comparative example is a hydroxy polyacrylate emulsion synthesized by reaction at 80° C. at normal pressure in step S5, and the specific steps are:
[0205] S1. In parts by mass, 5.7 parts of acrylic acid, 5.5 parts of cyclohexyl methacrylate, 10 parts of methyl methacrylate, 5 parts of butyl acrylate, 7 parts of styrene, 10 parts of hydroxyethyl methacrylate, and 15 parts of epoxy soybean oil GreenSoft H were mixed to form a mixed solution A7 for standby use;
[0206] S2. Add 33 parts of deionized water to the dispersion tank, dissolve 0.5 parts of SDS and 1 part of EH-9, stir well and adjust the disperser to 700 rpm, add 58.2 parts of the mixture A7, drip it for 25 minutes, continue to disperse for 10 minutes after dripping, and obtain the pre-emulsion B7 standby;
[0207] S3. In parts by mass, 0.45 parts of APS and 1 part of COPS-1 were dissolved in 7 parts of deionized water to form a mixed solution C7 for standby use;
[0208] S4. In parts by mass, 8.5 parts of deionized water and 0.6 parts of DMEA were mixed to form a mixed solution D7 for standby use;
[0209] S5. Add 19.95 parts of deionized water, 0.25 parts of SDS, 0.5 parts of EH-9, 0.2 parts of Na2CO3 and 0.15 parts of APS to a four-necked flask equipped with a thermometer, a condenser, a stirring paddle and a constant pressure dropping funnel, mix and heat, and when the temperature reaches 77°C, add 9.3 parts of pre-emulsion B7 dropwise over 15 minutes, and stabilize for 10 minutes after the addition to obtain a seed emulsion. Raise the temperature to 80°C, and simultaneously add 83.4 parts of pre-emulsion B7 and 8.45 parts of mixed solution C7 dropwise over 3.5 hours, and then raise the temperature to 85°C after the addition, keep warm for 2 hours, cool to 55°C, add 9.1 parts of mixed solution D7, stir for 10 minutes, and keep warm at 80°C for 60 minutes at normal pressure. The epoxy value is 0.1 as determined by the hydrochloric acid-acetone method, and the epoxy soybean oil does not undergo polycondensation with the hydroxy acrylate polymer;
[0210] S6. Cool down to 40° C., release the pressure, and filter the material to obtain the bio-based hydroxy polyacrylate emulsion 7.
[0211] Comparative Example 8
[0212] A water-based two-component polyurethane coating 7 was prepared in the comparative example. The emulsion was prepared in the comparative example 7. The specific steps were as follows:
[0213] During construction, mix A7 and B7 agents at a NCO / OH molar ratio of 1.8:1;
[0214] Wherein, the A7 agent comprises the following components in parts by weight:
[0215]
[0216] Agent B7 is a water-based polyisocyanate curing agent, the water-based polyisocyanate curing agent is Bayhydur XP2487 / 1, and the mass fraction of Bayhydur XP 2487 / 1 is 13.4 parts;
[0217] The preparation method of the A7 agent of the above-mentioned bio-based water-based two-component polyurethane coating 7 is as follows: add the bio-based hydroxy polyacrylate emulsion 7 into a stirring tank at a rotation speed of 700 rpm, premix water, dipropylene glycol butyl ether and dipropylene glycol methyl ether and add them into the stirring tank, add TEGO-800, RM-8W, TEGO-245 and TEA in sequence, disperse for 20 minutes, and filter the material.
[0218] During construction, agent B7 was added to agent A7 and stirred for 6 minutes to obtain a bio-based waterborne two-component polyurethane coating 7, whose bio-based content was 15.3%.
[0219] The paint film prepared from the bio-based waterborne two-component polyurethane coating 7 was cured and dried at room temperature for 7 days, and its properties are shown in Table 7.
[0220] Test Example 1
[0221] The water-based two-component polyurethane coatings prepared in the examples and comparative examples were cured and dried at room temperature for 7 days, and their properties are shown in Table 1.
[0222] The test standards are:
[0223] Coating appearance: visual inspection;
[0224] Surface drying time: GB / T1728-2020;
[0225] Drying time: GB / T1728-2020;
[0226] Pencil hardness: GB / T6739-2006;
[0227] Coating gloss / (60°,%): GB / T9754-2007;
[0228] Water resistance (25℃, 24h): GB / T4893.1-2020;
[0229] Dry heat resistance (70±2℃, 15h): GB / T4893.3-2020;
[0230] Ethanol resistance (50%, 1h): GB / T4893.1-2020;
[0231] The detection method is as follows:
[0232] Basic performance tests include: Bio-based hydroxy polyacrylate emulsions are tested in accordance with GB / T11175-2002 "Test Methods for Synthetic Resin Emulsions", and the appearance, pH, solid content, viscosity, and gel fraction (coarse particles) of the emulsions are tested. Paint film performance is tested in accordance with GB / T23999-2009 "Water-based Wood Coatings for Interior Decoration and Renovation", and the gloss, hardness, water resistance, dry heat resistance, and alcohol resistance are tested. The average particle size of the emulsion is measured using a nanoparticle size analyzer (ZS Nano S).
[0233] Table 1 Comprehensive properties of bio-based waterborne two-component polyurethane coating 1
[0234]
[0235]
[0236] It can be seen from the above table that the water-based two-component polyurethane coating 4 of comparative examples 2, 4, 6, and 8 has a longer surface drying time than the bio-based water-based two-component polyurethane coating 1 of Example 2, which is not conducive to improving construction efficiency, and is far inferior to the example in terms of paint film pencil hardness, water resistance, dry heat resistance, and ethanol resistance; the present invention discloses a method for preparing a bio-based hydroxy polyacrylate emulsion. The bio-based hydroxy polyacrylate emulsion prepared by the preparation method has a high hydroxyl content, good appearance and good stability; the paint film made of the prepared bio-based water-based two-component polyurethane coating has the advantages of high hardness, excellent water resistance and chemical resistance, high crosslinking density, scratch resistance, wear resistance and fast drying speed, and can be applied to high-end wood coatings, automotive coatings, metal anti-corrosion coatings and other industrial protective coatings.
[0237] Test Example 2
[0238] This test example tested the properties of the emulsions in Examples 1, 3, 5 and Comparative Examples 1, 3, 5 and 7. The data results are shown in Table 2.
[0239] Table 2: Emulsion performance comparison table
[0240]
[0241]
[0242] The difference between Comparative Example 1 and Example 1 is that the hydroxy polyacrylate emulsion synthesized without adding bio-based materials. Compared with Example 1, the bio-based content of Comparative Example 1 is 0%, the pH is acidic, the hydroxyl content is low, the solid content is low, and the thermal storage stability is poor. The reason for the above problems is that the carboxyl reaction of epoxy soybean oil and hydroxy polyacrylate polymer is not added, and the residual carboxyl content of the polymer is too high. Comparative Example 3 is a hydroxy polyacrylate emulsion synthesized according to the conventional process without adding bio-based materials, and its hydroxyl content and solid content parameters are consistent with Example 1. Compared with Example 1, the bio-based content of Comparative Example 3 is 0%, the appearance is slightly poor, the particle size is large, the thermal storage stability is poor, and the high gel rate indicates poor polymerization stability. The cause of the above problems is that the amount of hydrophilic hydroxy acrylate monomer added is too high. Comparative Example 5 does not add hydroxy acrylate monomer, and its hydroxyl group is only generated by the reaction of hydrophilic modified epoxy soybean oil with secondary amino groups. Its hydroxyl group is only generated by the reaction of epoxy soybean oil with carboxyl groups. Compared with Example 1, the bio-based content of Comparative Example 5 is higher, at 51.9%, but the thermal storage stability is poor. In addition, the high gel rate indicates that the polymerization stability is poor. The reason for the above problems is that the amount of epoxidized soybean oil added is too high and the cross-linking density of the polymer is too large. Comparative Example 7 changes the high temperature and high pressure reaction of Example 1 to a hydroxy polyacrylate emulsion synthesized by a reaction at normal pressure and 80°C. Its bio-based content, solid content, appearance, and particle size are consistent with those of Example 1, but the pH is acidic and the hydroxyl content is low. The reason for the above problems is that the epoxy group of the epoxidized soybean oil did not react with the carboxyl group of the hydroxy polyacrylate polymer under normal pressure and 80°C.
[0243] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
Claims
1. A bio-based hydroxy polyacrylate emulsion, characterized in that: The preparation raw materials include: bio-based materials and polymerized monomers; The bio-based material is a bio-based oil containing epoxy groups; The polymerizable monomers include hydroxy acrylate monomers, acrylic acid monomers, acrylate monomers and vinyl monomers; The acrylic acid monomer includes at least one of an acrylic acid monomer and a methacrylic acid monomer; The acrylic acid ester monomer comprises at least one of methyl methacrylate, butyl acrylate, isobornyl acrylate, cyclohexyl methacrylate and benzyl methacrylate; The vinyl monomer includes styrene; The hydroxy acrylate monomer includes at least one of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate and hydroxypropyl methacrylate; The preparation method of the bio-based hydroxy polyacrylate emulsion comprises: S1: 4 to 7 parts of acrylic acid monomer, 15 to 35 parts of acrylic acid ester monomer, 5 to 10 parts of vinyl monomer, 5 to 15 parts of hydroxy acrylic acid ester monomer and 9 to 15 parts of bio-based material are mixed to form a mixed solution A for use; S2: 28-33 parts of deionized water, 0.45-2.1 parts of emulsifier, and 55.75-60.8 parts of mixed solution A are mixed to obtain a pre-emulsified solution B for use; S3: 5-7 parts of deionized water, 0.2-0.6 parts of initiator and 0-1 parts of emulsifier are mixed to obtain a mixed solution C for standby use; S4: 5 to 8.5 parts of deionized water and 0.5 to 0.7 parts of neutralizer 1 are mixed to form a mixed solution D for later use; S5: deionized water, an emulsifier and a buffer are mixed, stirred and heated, and then part of the pre-emulsion B is added to obtain a seed emulsion, and then the remaining pre-emulsion B and mixed solutions C and D are added to react to obtain a bio-based hydroxy polyacrylate emulsion; In step S5, by weight, the mixture includes 19 to 25 parts of deionized water, 0.3 to 0.8 parts of an emulsifier, 0.1 to 0.5 parts of a buffer, 83 to 96 parts of a pre-emulsified solution B, 5.5 to 8.5 parts of a mixed solution C, and 5.5 to 9.5 parts of a mixed solution D; The preparation method comprises mixing and reacting the bio-based material and a polyacrylate polymer containing hydroxyl groups, wherein the reaction temperature is 150-170° C. and the reaction pressure is 1.9-2.5 MPa; The bio-based content of the bio-based hydroxy polyacrylate emulsion is 5% to 25%; The mass content of hydroxyl groups in the bio-based hydroxy polyacrylate emulsion is 2.5% to 4.6%.
2. The bio-based hydroxy polyacrylate emulsion according to claim 1, characterized in that The particle size of the bio-based hydroxy polyacrylate emulsion is 80nm~120nm.
3. The bio-based hydroxy polyacrylate emulsion according to claim 1, characterized in that The bio-based hydroxy polyacrylate emulsion has a solid content of 47-52% by weight.
4. A coating, characterized in that: The raw material for preparing the coating includes the bio-based hydroxy polyacrylate emulsion according to any one of claims 1 to 3.
5. Use of the coating according to claim 4 in the field of decoration.