Quaternary copolymer polyamide PA56IT and preparation method thereof
By designing quaternary copolymer polyamide PA56IT, the problem of insufficient transparency and mechanical properties of existing transparent plastics in specific fields is solved, and polyamides with high light transmittance and excellent mechanical properties are achieved, which expands its application range and simplifies production Craft.
Patent Information
- Application Number
- CN202110894844.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-05
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-08-05
AI Technical Summary
Existing transparent plastics such as PC and PMMA have small molecule residues, poor chemical corrosion resistance, and poor wear resistance during use. In addition, ordinary polyamides have poor transparency due to regular molecular chain arrangement, making them difficult to play a role in specific fields.
By designing quaternary copolyamide PA56IT, controlling the chain distribution and amorphous properties of amide bonds, polyamides with high light transmittance and excellent mechanical properties are prepared, using specific monomer ratios and process conditions, including pentyldiamine and hexadecano. Molar ratios of diamine, terephthalic acid and isophthalic acid, as well as additives such as capping agents and UV stabilizers, optimize the structure and properties of the polyamide.
The high transparency and excellent mechanical properties of polyamide are achieved, making it used in harsh environments, expanding the application range of transparent polyamides, simplifying the preparation process, and reducing raw material costs.
Smart Images

Figure BDA0003197475040000021 
Figure BDA0003197475040000111 
Figure FDA0004926121760000011
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer materials, and specifically relates to a quaternary copolymer polyamide PA56IT with high light transmittance and excellent mechanical properties, and a preparation method and application thereof. Background Art
[0002] Polyamide has excellent mechanical properties and molding properties, and is widely used in the processing of automotive parts, parts of electrical and electronic equipment, eyeglass frames, eyeglass lenses or other lenses, cups / bottles for drinking water treatment, etc. However, ordinary polyamide has poor transparency due to its regular molecular chain arrangement, so it is difficult to play a role in special fields.
[0003] In actual use, traditional transparent plastics cannot fully meet the requirements of specific use scenarios. For example, the main transparent plastics PC (polycarbonate) and PMMA (polymethyl methacrylate) on the market have small molecule residues, poor chemical corrosion resistance, and poor wear resistance. Polyamide macromolecules contain highly polar amide groups, as well as terminal amino and carboxyl groups. These groups have strong interactions and are very easy to form hydrogen bonds, which makes them highly crystallized. The size of the spherulites formed by polyamide is often relatively large, larger than the wavelength of visible light (400-700nm), resulting in its opacity. In order to prepare polyamide with higher transparency, it is possible to prepare amorphous polyamide by reducing the crystallinity; reduce the crystal size to within the visible light wavelength range; optimize blending, copolymerization and other methods to make the refractive index of the crystalline region and the amorphous region similar, etc., but these methods may cause the loss of other properties. For example, inhibiting crystallization will cause the hardness of polyamide to decrease, the heat deformation temperature to decrease, and even lose its use value. In addition, some commercially available transparent polyamides often use cyclic lipid amines with side groups, which are often expensive. Summary of the invention
[0004] The purpose of the present invention is to provide a tetrapolymer polyamide PA56IT which can be used to prepare a tetrapolymer polyamide having high light transmittance and transparency, excellent mechanical properties and economical and practical properties, and a preparation method and application thereof by specifying the chain distribution and amorphous characteristics of the amide bonds in the tetrapolymer polyamide.
[0005] The present invention provides a quaternary copolymer polyamide PA56IT, wherein the quaternary copolymer polyamide PA56IT comprises structural units represented by formulas (I), (II) and (III):
[0006]
[0007] Among them, in the quaternary copolymer polyamide PA56IT,
[0008] The molar fraction of structural unit (I) is 20 to 60 parts;
[0009] The molar fraction of structural unit (II) is 0 to 25 parts;
[0010] The molar fraction of structural unit (III) is 35 to 60 parts;
[0011] The molar fraction of the structural unit (IV) is 1 to 30 parts;
[0012] The total molar fraction of the structural units (I), (II), (III) and (IV) is 100 parts;
[0013] Preferably, the content of the structural units (I), (II), (III) and (IV) in the tetrapolymer polyamide PA56IT is above 95%, preferably above 97%.
[0014] In one embodiment, the ratio of the sum of the molar fractions of the structural units (I) and (II) to the sum of the molar fractions of the structural units (III) and (IV) is 1:0.95-1.07;
[0015] Preferably, the molar fraction of the structural unit (I) is 30 to 50 parts, for example, 30 parts, 35 parts, 40 parts, 45 parts, 48 parts, 50 parts;
[0016] Preferably, the molar fraction of the structural unit (II) is 0 to 20 parts, such as 5 parts, 10 parts, 15 parts;
[0017] Preferably, the molar ratio of the structural units (I) to (II) is 3-5:0.01-2;
[0018] Preferably, the molar ratio of the structural units (I) to (III) is 3-5:4-5;
[0019] Preferably, the molar ratio of the structural units (I), (II) and (III) is 3-5:0.01-2:4-5.
[0020] Preferably, the molar fraction of the structural unit (I) is 60-100%, such as 70%, 80%, or 90%, relative to the total molar fraction of the structural units (I) and (II).
[0021] In one embodiment, the number average molecular weight of the quaternary copolymer polyamide PA56IT is 10,000 to 50,000, for example, 20,000 to 30,000; and / or,
[0022] The relative viscosity of the quaternary copolymer polyamide PA56IT is 1.60 to 3.0, preferably 1.8 to 2.7, for example 1.8 to 2.3; and / or,
[0023] The glass transition temperature of the quaternary copolymer polyamide PA56IT is 128-145° C., preferably 129-142° C.; and / or,
[0024] The tensile strength of the quaternary copolymer polyamide PA56IT is 80 to 130 MPa, preferably 90 to 100 MPa; and / or,
[0025] The flexural strength of the quaternary copolymer polyamide PA56IT is 140 to 175 MPa, preferably 145 to 155 MPa; and / or,
[0026] The IZOD notched impact strength of the quaternary copolymer polyamide PA56IT is 7.0 to 12.0 KJ / m 2 , preferably 8.0~9.0KJ / m 2 and / or,
[0027] The haze of the quaternary copolymer polyamide PA56IT is less than 6.0%, preferably less than 4.5%; and / or,
[0028] The light transmittance of the tetrapolymer polyamide PA56IT is 85% or more, and preferably 90% or more.
[0029] In one embodiment, the quaternary copolymer polyamide PA56IT further comprises additives, the additives comprising end-capping agents, UV stabilizers, heat stabilizers, free radical scavengers and / or processing aids, impurity inhibitors, lubricants, demoulding aids, plasticizers, functional additives for influencing optical properties, in particular refractive index, impact modifiers, nanofillers and / or additives, brighteners, dyes or mixtures thereof; and / or,
[0030] The content of the additive in the tetrapolymer polyamide PA56IT is 5% or less, and preferably 3% or less. The percentage is a mass percentage.
[0031] In one embodiment, the raw materials of the quaternary copolymer polyamide PA56IT include the following monomers:
[0032] 35-60 parts of pentamethylenediamine;
[0033] 1-30 parts of hexamethylenediamine;
[0034] 0 to 25 parts of terephthalic acid and / or its derivatives, more preferably 0 to 20 parts;
[0035] 20 to 60 parts of isophthalic acid and / or its derivatives, more preferably 30 to 55 parts;
[0036] All parts are calculated on a molar basis.
[0037] In one embodiment, the pentamethylenediamine is pentamethylenediamine of chemical or biological origin, preferably pentamethylenediamine of biological origin; and / or,
[0038] The terephthalic acid derivative is selected from one or more of terephthaloyl chloride, dimethyl terephthalate and diethyl terephthalate; and / or,
[0039] The isophthalic acid derivative is selected from one or more of isophthaloyl chloride, dimethyl isophthalate and diethyl isophthalate.
[0040] In one embodiment, the raw materials of the quaternary copolymer polyamide PA56IT further include additives, the additives including end capping agents, UV stabilizers, heat stabilizers, free radical scavengers and / or processing aids, impurity inhibitors, lubricants, demoulding aids, plasticizers, functional additives for affecting optical properties, especially refractive index, impact modifiers, nanofillers and / or additives, brighteners, dyes or mixtures thereof.
[0041] In one embodiment, the capping agent preferably includes any one or more of a monoacid, a diacid, a monoamine or a diamine, and further preferably includes one or more of acetic acid, benzoic acid, stearic acid, lauric acid, succinic acid, adipic acid, sebacic acid, undecanedicarboxylic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecanedicarboxylic acid, hexadecanedioic acid, and one or more of decylamine, dodecylamine, hexamethylenediamine, and decanediamine.
[0042] In one embodiment, the heat stabilizer preferably includes one or more of phosphoric acid, phosphorous acid, trimethyl phosphite, triphenyl phosphite, trimethyl phosphate, triphenyl phosphate, sodium hypophosphite, zinc hypophosphite, calcium hypophosphite, and potassium hypophosphite.
[0043] In one embodiment, the crystallization promoter preferably includes a long carbon chain carboxylic acid metal salt, the number of carbon atoms of the long carbon chain carboxylic acid is preferably 10 to 30, and the metal preferably includes one or more of calcium, magnesium, and zinc, for example, it can be a long carbon chain carboxylic acid calcium salt, a long carbon chain carboxylic acid magnesium salt or a long carbon chain carboxylic acid zinc salt, and further can be one or more of calcium dodecanoate, sodium myristate, calcium heptadecanoate, calcium octadecanoate, sodium dodecyl sulfate, and sodium myristate.
[0044] In one embodiment, the inorganic filler preferably includes one or more of glass fiber, glass beads, carbon fiber, carbon black, and graphite.
[0045] In one embodiment, the mineral preferably includes one or more additives selected from titanium dioxide, calcium carbonate and barium sulfate.
[0046] On the other hand, the present invention provides a method for preparing the above-mentioned quaternary copolymer polyamide PA56IT, which comprises the following steps: mixing pentamethylenediamine, hexamethylenediamine, terephthalic acid and / or its derivatives, isophthalic acid and / or its derivatives with water in a molar ratio to obtain a polyamide salt solution; adjusting the pH of the polyamide salt solution so that the pH value of the polyamide salt solution is above 8.0 when the concentration is 10%, raising the temperature so that the pressure in the reaction system is 0.3-3.2 MPa, for example, 1.7 MPa, 2.0 MPa, maintaining the pressure for 30-120 min, for example, 50 min, and then releasing the pressure to normal pressure; evacuating the reaction system for 20-100 min, for example, 30 min, 40 min, and the temperature after the reaction is 230-290° C., for example, 240° C., 260° C., 280° C., to obtain a melt; discharging the melt, drawing and pelletizing to obtain PA56IT resin.
[0047] In one embodiment, the ratio of the sum of the moles of terephthalic acid and / or its derivatives and isophthalic acid and / or its derivatives to the sum of the moles of pentamethylenediamine and hexamethylenediamine is 1:0.95-1.07, for example 1:1;
[0048] Preferably, the molar ratio of isophthalic acid and / or its derivatives, terephthalic acid and / or its derivatives to pentamethylenediamine is 3-5:0.01-2:4-5;
[0049] Preferably, the molar number of the isophthalic acid and / or its derivatives is 60 to 100% of the sum of the molar numbers of terephthalic acid and / or its derivatives and isophthalic acid and / or its derivatives.
[0050] In one embodiment, the method is performed under nitrogen or an inert gas atmosphere, wherein the inert gas includes argon or helium.
[0051] In one embodiment, the concentration of the polyamide salt solution is between 40% and 85%, where the percentage is the mass percentage of the polyamide PA56IT salt solution, such as 50% or 60%.
[0052] In one embodiment, the polyamide salt solution can be concentrated by heating to increase the concentration.
[0053] In one embodiment, the pH value is 8.0-9.0, such as 8.3, 8.4, 8.5, and the percentage is the mass percentage of the polyamide PA56 IT salt solution.
[0054] In one embodiment, the aforementioned additives are added to the polyamide salt solution, and the additives are added in an amount of 100-2000 ppm (calculated based on the total mass of the raw materials). For example, when the raw materials are pentamethylenediamine, terephthalic acid and isophthalic acid, the additives are added in an amount of 100-2000 ppm based on the total mass of the raw materials.
[0055] In one embodiment, the aforementioned antioxidant is added to the polyamide salt solution, and the amount of the additive added is 200-1500 ppm (calculated based on the total mass of the raw materials), for example, 300 ppm, 700 ppm.
[0056] In one embodiment, the aforementioned end-capping agent is added to the polyamide salt solution, and the amount of the end-capping agent added is 100-1500 ppm (calculated based on the total mass of the raw materials), for example, 100 ppm.
[0057] In another aspect of the present invention, a molded product is provided, wherein the raw material of the molded product comprises any of the above-mentioned quaternary copolymer polyamide PA56IT.
[0058] Compared with the prior art, the implementation of the present invention has at least the following advantages:
[0059] 1. The quaternary copolymer polyamide PA56IT synthesized in the present invention not only has good transparency and light transmittance, but also has excellent mechanical properties, so that it can be used in more demanding use environments, which to a certain extent expands the use scope of transparent polyamide.
[0060] 2. The preparation method of the quaternary copolymer polyamide PA56IT of the present invention is simple, the raw material price is cheap, the process parameters are easy to control, and it is convenient for quantitative production. DETAILED DESCRIPTION
[0061] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0062] The inventors of the present application selected bio-based pentamethylenediamine containing an odd number of carbon atoms, and simultaneously introduced a benzene ring structure into the molecular chain, controlling the content ratio of the monomers. Unexpectedly, they found that the obtained polyamide not only has high transparency, but also has excellent mechanical properties such as tensile strength, flexural strength, and impact toughness, enabling it to meet the needs of different transparent products.
[0063] The polyamide according to one embodiment of the present invention and its preparation are further described below in conjunction with specific examples.
[0064] The relevant tests involved are as follows:
[0065] 1) Bending test: The test is based on ISO 178-2010, test conditions: 2 mm / min, sample size: 10 mm*4 mm*80 mm.
[0066] 2) Tensile test: The test reference standard ISO 572-2-2012, test conditions: 50 mm / min.
[0067] 3) Impact test: Izod beam notched impact test, refer to test standard ISO 180 / 1A, test condition 23°C.
[0068] 4) Transmittance and haze: The test refers to the national standard GB / T 2410-2008, with a thickness of 2mm.
[0069] 5) Relative viscosity: by Ubbelohde viscometer concentrated sulfuric acid method: accurately weigh 0.25±0.0002g of the dried polyamide resin slices, add 50mL of concentrated sulfuric acid (96wt%) to dissolve; measure and record the concentrated sulfuric acid flow time t0 and the polyamide sample solution flow time t in a 25℃ constant temperature water bath. Viscosity calculation formula: relative viscosity = t / t0; t—solution flow time; t0—solvent flow time.
[0070] 6) Glass transition temperature (Tg): refers to the temperature corresponding to the transition from glassy state to highly elastic state, and is measured using differential scanning calorimetry.
[0071] Pentamethylenediamine was purchased from Cathay (Jinxiang) Biomaterial Co., Ltd., and hexamethylenediamine, terephthalic acid, and isophthalic acid were purchased from Sinopharm Chemical Reagent Co., Ltd. Other raw materials and reagents can be prepared by methods known in the literature or purchased commercially.
[0072] Example 1
[0073] 1. Under nitrogen conditions, isophthalic acid, terephthalic acid, pentamethylenediamine, hexamethylenediamine and water are mixed evenly, wherein the molar proportion is isophthalic acid: terephthalic acid: pentamethylenediamine: hexamethylenediamine = 30:20:40:10, to obtain a 50% polyamide salt solution, pentamethylenediamine is used to adjust the pH value of the solution, so that the pH value is 8.3 when it is diluted to 10wt%, and 300ppm of antioxidant sodium hypophosphite is added.
[0074] 2. The obtained salt solution was heated until the pressure in the reaction system reached 1.7 MPa. After maintaining the pressure for 50 minutes, the pressure was released until it reached normal pressure.
[0075] 3. After the reaction system is depressurized to normal pressure, vacuum is performed. The whole process lasts for 30 minutes, and the material temperature after vacuuming is controlled to be 240°C.
[0076] 4. The material is melted, drawn into strands and pelletized to obtain a transparent polyamide resin. The performance test is shown in Table 1.
[0077] Example 2
[0078] The preparation method of the transparent polyamide resin is the same as that of Example 1, except that the raw materials in step 1 are: isophthalic acid, terephthalic acid, pentamethylenediamine and water are uniformly mixed, wherein the molar proportion is isophthalic acid: terephthalic acid: pentamethylenediamine: hexamethylenediamine = 35:15:45:5. The transparent polyamide resin is obtained, and the performance test is shown in Table 1.
[0079] Example 3
[0080] 1. Under nitrogen conditions, isophthalic acid, terephthalic acid, pentamethylenediamine, hexamethylenediamine and water are mixed evenly, wherein the molar proportion is isophthalic acid: terephthalic acid: pentamethylenediamine: hexamethylenediamine = 40:10:48:2, to obtain a polyamide salt solution with a concentration of 60%, and pentamethylenediamine is used to adjust the pH value of the solution to 8.4 when it is diluted to 10wt%, and 700ppm of antioxidant calcium hypophosphite is added.
[0081] 2. The obtained salt solution was heated until the pressure in the reaction system reached 1.7 MPa. After maintaining the pressure for 45 minutes, the pressure was released until it reached normal pressure.
[0082] 3. After the reaction system is depressurized to normal pressure, vacuum is performed. The whole process lasts for 40 minutes, and the material temperature after vacuuming is controlled to be 240°C.
[0083] 4. The material is melted, drawn into strands and pelletized to obtain a transparent polyamide resin. The performance test is shown in Table 1.
[0084] Example 4
[0085] The preparation method of the transparent polyamide resin is the same as that of Example 3, except that the raw materials in step 1 are: isophthalic acid, terephthalic acid, pentamethylenediamine and water are uniformly mixed, wherein the molar proportion is isophthalic acid: terephthalic acid: pentamethylenediamine: hexamethylenediamine = 45:5:45:5. A transparent polyamide resin is obtained, and the performance test is shown in Table 1.
[0086] Example 5
[0087] 1. Under nitrogen conditions, isophthalic acid, pentamethylenediamine, hexamethylenediamine and water are mixed evenly, wherein the molar ratio is isophthalic acid: pentamethylenediamine: hexamethylenediamine = 50:45:5, to obtain a polyamide salt solution with a concentration of 60%. Pentamethylenediamine is used to adjust the pH value of the solution so that the pH value is 8.4 when it is diluted to 10wt%, and 700ppm of antioxidant calcium hypophosphite is added.
[0088] 2. The obtained salt solution is heated until the pressure in the reaction system reaches 2.0 MPa. After maintaining the pressure for 50 minutes, the pressure is released until it reaches normal pressure.
[0089] 3. After the reaction system is depressurized to normal pressure, vacuum is performed. The whole process lasts for 30 minutes, and the material temperature after vacuuming is controlled to be 260°C.
[0090] 4. The material is melted, drawn into strands and pelletized to obtain a transparent polyamide resin. The performance test is shown in Table 1.
[0091] Example 6
[0092] 1. Under nitrogen conditions, isophthalic acid, terephthalic acid, pentamethylenediamine, hexamethylenediamine and water are mixed evenly, wherein the molar ratio is isophthalic acid: terephthalic acid: pentamethylenediamine: hexamethylenediamine = 48:2:45:5, to obtain a 50% polyamide salt solution, pentamethylenediamine is used to adjust the pH value of the solution, so that the pH value is 8.5 when it is diluted to 10wt%, and 300ppm of antioxidant calcium hypophosphite is added.
[0093] 2. The obtained salt solution was heated until the pressure in the reaction system reached 1.7 MPa. After maintaining the pressure for 50 minutes, the pressure was released until it reached normal pressure.
[0094] 3. After the reaction system is depressurized to normal pressure, vacuum is performed. The whole process lasts for 30 minutes, and the material temperature after vacuuming is controlled to be 280°C.
[0095] 4. The material is melted, drawn into strands and pelletized to obtain a transparent polyamide resin. The performance test is shown in Table 1.
[0096] Example 7
[0097] 1. Under nitrogen conditions, isophthalic acid, terephthalic acid, pentamethylenediamine, hexamethylenediamine and water are mixed evenly, wherein the molar proportion is isophthalic acid: terephthalic acid: pentamethylenediamine: hexamethylenediamine = 48:2:45:5, to obtain a 50% polyamide salt solution, pentamethylenediamine is used to adjust the pH value of the solution to 8.5 when it is diluted to 10wt%, and 300ppm of antioxidant calcium hypophosphite and 100ppm of end-capping agent acetic acid are added.
[0098] 2. The obtained salt solution was heated until the pressure in the reaction system reached 1.7 MPa. After maintaining the pressure for 50 minutes, the pressure was released until it reached normal pressure.
[0099] 3. After the reaction system is depressurized to normal pressure, vacuum is performed. The whole process lasts for 40 minutes, and the material temperature after vacuuming is controlled to be 280°C.
[0100] 4. The material is melted, drawn into strands and pelletized to obtain a transparent polyamide resin. The performance test is shown in Table 1.
[0101] Comparative Example 1
[0102] 1. Under nitrogen conditions, isophthalic acid, terephthalic acid, pentamethylenediamine, hexamethylenediamine and water are mixed evenly, wherein the molar proportion is isophthalic acid: terephthalic acid: pentamethylenediamine: hexamethylenediamine = 25:25:38:12, to obtain a 50% polyamide salt solution, pentamethylenediamine is used to adjust the pH value of the solution to 8.5 when it is diluted to 10wt%, and 700ppm of antioxidant calcium hypophosphite is added.
[0103] 2. The obtained salt solution was heated until the pressure in the reaction system reached 1.7 MPa. After maintaining the pressure for 50 minutes, the pressure was released until it reached normal pressure.
[0104] 3. After the reaction system is depressurized to normal pressure, vacuum is performed. The whole process lasts for 40 minutes, and the material temperature after vacuuming is controlled to be 240°C.
[0105] 4. The material is melted, drawn into strands and pelletized to obtain polyamide resin. The performance test is shown in Table 1.
[0106] Comparative Example 2
[0107] 1. Under nitrogen conditions, isophthalic acid, terephthalic acid, pentamethylenediamine, hexamethylenediamine and water are mixed evenly, wherein the molar proportion is isophthalic acid: terephthalic acid: pentamethylenediamine: hexamethylenediamine = 28:22:33:17, to obtain a 50% polyamide salt solution, pentamethylenediamine is used to adjust the pH value of the solution, so that the pH value is 8.5 when it is diluted to 10wt%, and 700ppm of antioxidant calcium hypophosphite is added.
[0108] 2. The obtained salt solution was heated until the pressure in the reaction system reached 1.7 MPa. After maintaining the pressure for 40 minutes, the pressure was released until it reached normal pressure.
[0109] 3. After the reaction system is depressurized to normal pressure, vacuum is performed. The whole process lasts for 38 minutes, and the material temperature after vacuuming is controlled to be 240°C.
[0110] 4. The material is melted, drawn into strands and pelletized to obtain polyamide resin. The performance test is shown in Table 1.
[0111] Table 1
[0112]
[0113] In summary, by comparison, the quaternary copolymer polyamide PA56IT of the present invention has very excellent comprehensive properties and has very broad application prospects in the field of general polyamides.
[0114] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A quaternary copolymer polyamide PA56IT, characterized in that: The tetrapolymer polyamide PA56IT comprises structural units represented by formulas (I), (II), (III) and (IV): Among them, in the quaternary copolymer polyamide PA56IT, The molar fraction of structural unit (I) is 20 to 60 parts; The molar fraction of structural unit (II) is 0 to 25 parts; The molar fraction of structural unit (III) is 35 to 60 parts; The molar fraction of the structural unit (IV) is 1 to 30 parts; The total molar fraction of the structural units (I), (II), (III) and (IV) is 100 parts; The content of the structural units (I), (II), (III) and (IV) in the tetrapolymer polyamide PA56IT is above 95%; The molar ratio of the structural units (I) to (II) is 3-5:0.01-2, and the molar ratio of the structural units (I) to (III) is 3-5:4; the relative viscosity of the quaternary copolymer polyamide PA56IT is 1.60-3.0, and the glass transition temperature of the quaternary copolymer polyamide PA56IT is 128-145°C.
2. The quaternary copolymer polyamide PA56IT according to claim 1, characterized in that: The ratio of the sum of the molar fractions of the structural units (I) and (II) to the sum of the molar fractions of the structural units (III) and (IV) is 1:0.95-1.07; and / or, The molar fraction of the structural unit (I) is 30 to 50 parts; and / or, The molar fraction of the structural unit (II) is 0 to 20 parts; and / or, The molar fraction of the structural unit (I) is 60 to 100% of the total molar fraction of the structural units (I) and (II); and / or, The content of the structural units (I), (II), (III) and (IV) in the tetrapolymer polyamide PA56IT is above 97%.
3. The quaternary copolymer polyamide PA56IT according to claim 1, characterized in that: The number average molecular weight of the quaternary copolymer polyamide PA56IT is 10000 to 50000; and / or, The relative viscosity of the quaternary copolymer polyamide PA56IT is 1.8 to 2.7; and / or, The glass transition temperature of the quaternary copolymer polyamide PA56IT is 129-142° C.; and / or, The tensile strength of the quaternary copolymer polyamide PA56IT is 80 to 130 MPa; and / or, The flexural strength of the quaternary copolymer polyamide PA56IT is 140 to 175 MPa; and / or, The IZOD notched impact strength of the quaternary copolymer polyamide PA56IT is 7.0 to 12.0 KJ / m 2 and / or, The haze of the tetrapolymer polyamide PA56IT is less than 6.0%; and / or, The light transmittance of the quaternary copolymer polyamide PA56IT is above 85%.
4. The quaternary copolymer polyamide PA56IT according to claim 1, characterized in that: The number average molecular weight of the quaternary copolymer polyamide PA56IT is 20000 to 30000; and / or, The tensile strength of the quaternary copolymer polyamide PA56IT is 90 to 100 MPa; and / or, The flexural strength of the quaternary copolymer polyamide PA56IT is 145-155 MPa; and / or, The IZOD notched impact strength of the quaternary copolymer polyamide PA56IT is 8.0 to 9.0 KJ / m 2 and / or, The haze of the quaternary copolymer polyamide PA56IT is less than 4.5%; and / or, The light transmittance of the quaternary copolymer polyamide PA56IT is above 90%.
5. The quaternary copolymer polyamide PA56IT according to claim 1, characterized in that: The quaternary copolymer polyamide PA56IT further comprises additives, wherein the additives comprise end-capping agents, free radical scavengers and / or processing aids, impurity inhibitors, functional additives for influencing optical properties, impact modifiers, nanofillers, brighteners, dyes or mixtures thereof; and / or, The content of the additive in the quaternary copolymer polyamide PA56IT is less than 5%.
6. The quaternary copolymer polyamide PA56IT according to claim 5, characterized in that: The processing aids include UV stabilizers, heat stabilizers, lubricants, demoulding aids, plasticizers or mixtures thereof; and / or, The optical property is a refractive index; and / or, The content of the additive in the quaternary copolymer polyamide PA56IT is less than 3%.
7. The quaternary copolymer polyamide PA56IT according to claim 1, characterized in that: The raw materials of the quaternary copolymer polyamide PA56IT include the following monomers: 35-60 parts of pentamethylenediamine; 1-30 parts of hexamethylenediamine; 0-25 parts of terephthalic acid and / or its derivatives; 20-60 parts of isophthalic acid and / or its derivatives; All parts are calculated on a molar basis.
8. The quaternary copolymer polyamide PA56IT according to claim 7, characterized in that: The terephthalic acid and / or its derivatives are in an amount of 0 to 20 parts, and the isophthalic acid and / or its derivatives are in an amount of 30 to 55 parts.
9. The quaternary copolymer polyamide PA56IT according to claim 7, characterized in that: The pentamethylenediamine is of chemical or biological origin; and / or, The terephthalic acid derivative is selected from one or more of terephthaloyl chloride, dimethyl terephthalate and diethyl terephthalate; and / or, The isophthalic acid derivative is selected from one or more of isophthaloyl chloride, dimethyl isophthalate and diethyl isophthalate.
10. The quaternary copolymer polyamide PA56IT according to claim 9, characterized in that: The pentamethylenediamine is pentamethylenediamine derived from biomass.
11. The quaternary copolymer polyamide PA56IT according to claim 7, characterized in that: The raw materials of the quaternary copolymer polyamide PA56IT also include additives, which include end-capping agents, free radical scavengers and / or processing aids, impurity inhibitors, functional additives for affecting optical properties, impact modifiers, nanofillers, brighteners, dyes or mixtures thereof.
12. The quaternary copolymer polyamide PA56IT according to claim 11, characterized in that: The processing aids include UV stabilizers, heat stabilizers, lubricants, demoulding aids, plasticizers or mixtures thereof; and / or, The optical property is the refractive index.
13. A method for preparing the quaternary copolymer polyamide PA56IT as claimed in any one of claims 1 to 12, characterized in that: The method comprises the following steps: mixing pentamethylenediamine, hexamethylenediamine, terephthalic acid and / or its derivatives, isophthalic acid and / or its derivatives with water according to a molar fraction ratio to obtain a polyamide salt solution; adjusting the pH of the polyamide salt solution so that the pH value of the polyamide salt solution is above 8.0 when the concentration is 10%, raising the temperature so that the pressure in the reaction system is 0.3-3.2 Mpa, maintaining the pressure for 30-120 minutes, and then releasing the pressure to normal pressure; vacuuming the reaction system for 20-100 minutes, after which the temperature is 230-290° C. to obtain a melt; discharging the melt, drawing and pelletizing to obtain PA56IT resin.
14. The method for producing tetrapolymer polyamide PA56IT according to claim 13, characterized in that: The ratio of the sum of the moles of terephthalic acid and / or its derivatives and isophthalic acid and / or its derivatives to the sum of the moles of pentamethylenediamine and hexamethylenediamine is 1:0.95-1.07; and / or, The molar ratio of isophthalic acid and / or its derivatives, terephthalic acid and / or its derivatives to pentamethylenediamine is 3-5:0.01-2:4-5; and / or, The molar number of the isophthalic acid and / or its derivatives is 60 to 100% of the total molar number of terephthalic acid and / or its derivatives and isophthalic acid and / or its derivatives.
15. A molded article, characterized in that: The raw material of the molded product comprises the tetrapolymer polyamide PA56IT as described in any one of claims 1 to 12.
Citation Information
Patent Citations
Heat-resistant polyamide material and preparation method thereof
CN111378120A
Polyamide copolymer 56TI with low water absorption rate as well as preparation method and application thereof
CN113121817A
Polyamide resin composition
JP2012031403A
Transparent polyamide moulding compositions with high tensile strain at break
US20180171074A1