ITO planar target and sintering method and sintering device thereof

By using sealing structure and spiral oxygen injection channels during the sintering of ITO targets, oxygen inflow is controlled to achieve specific oxygen partial pressure, and the problem of large oxygen consumption is solved, and low oxygen consumption and high-density target sintering is achieved Effect.

CN115896724BActive Publication Date: 2024-11-19XIANDAO THIN FILM MATERIALS GUANGDONG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211636060.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-15
Publication Date
2024-11-19
Estimated Expiration
2042-12-15

AI Technical Summary

Technical Problem

The existing ITO target sintering methods consume a lot of oxygen, resulting in waste of oxygen and high production costs.

Method used

Using a sealed structure, the oxygen partial pressure test probe and spiral oxygen injection channel are used to control the inflow of oxygen to reach 30% to 90% oxygen partial pressure, avoid oxygen outflow, and sintering in a confined space to reduce the Oxygen consumption.

Benefits of technology

It significantly reduces oxygen waste during sintering, increases the density of the target material and reduces warpage, reduces oxygen consumption, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004001660960000011
    Figure HDA0004001660960000011
  • Figure HDA0004001660960000012
    Figure HDA0004001660960000012
Patent Text Reader

Abstract

The present invention belongs to the field of ITO target materials, and specifically discloses an ITO planar target and a sintering method and a sintering device thereof. In the sintering method of the present invention, the ITO planar target blank is sintered in a closed space suitable for its size, and the temperature and gas distribution in the space are more uniform, which can improve the density of the target material and reduce the warpage of the target material. At the same time, the sintering method of the present invention is carried out in a closed structure, which prevents oxygen from flowing out, so that after the oxygen partial pressure meets the conditions for suppressing the volatilization of the target material, it is no longer necessary to introduce oxygen, which greatly reduces the oxygen waste in the sintering process, and the oxygen consumption required for the overall sintering process is extremely low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of ITO target materials, and in particular relates to an ITO plane target and a sintering method and a sintering device thereof. Background Art

[0002] As one of the main raw materials for magnetron sputtering coating, ITO (indium tin oxide) targets are widely used in LCD, OLED, solar heterojunction cells and other fields due to the excellent conductivity, visible light transmittance and selective absorption of different wavelengths of the sputtered films. As the application fields of ITO targets continue to expand, its global demand is also growing.

[0003] The sintering methods of ITO targets include atmospheric pressure sintering, hot pressing sintering, microwave sintering, etc. Among them, atmospheric pressure sintering has the advantages of high production capacity and low equipment requirements and has become the main sintering method of ITO targets. As an indispensable sintering environment in atmospheric pressure sintering, the oxidizing atmosphere mainly suppresses the volatilization of indium oxide and tin oxide during the sintering process to ensure the normal progress of the sintering process. However, during the sintering process, oxygen needs to be continuously introduced to maintain the oxidizing atmosphere in the sintering furnace, resulting in oxygen being continuously discharged from the sintering furnace and wasted. The oxygen consumption in the sintering process accounts for a relatively large proportion of the production cost, so it is necessary to find a sintering method that can make full use of oxygen to reduce oxygen consumption and thus reduce production costs. Summary of the invention

[0004] In view of the problem of high oxygen consumption in the sintering method of conventional ITO target materials involved in the above-mentioned prior art, the present invention provides an ITO planar target and a sintering method and a sintering device thereof.

[0005] In order to achieve the above purpose, the following technical solutions are adopted:

[0006] A sintering method for an ITO planar target comprises the following steps:

[0007] (1) placing the ITO planar target blank in a sintering device for degreasing;

[0008] (2) A sealing structure is provided in the sintering device so that the degreased ITO planar target blank is placed in the sealing structure, wherein the sealing structure includes an oxygen partial pressure test probe and an oxygen injection channel; the temperature is then increased to 600-800°C at a heating rate of 1-5°C / min and kept warm, and oxygen is introduced through the oxygen injection channel during the insulation process. When the oxygen partial pressure reaches 30%-90%, the introduction of oxygen is stopped and the insulation at this temperature is terminated; the temperature is then increased to the sintering temperature for sintering, and the temperature is lowered to room temperature after the sintering is completed to obtain an ITO planar target.

[0009] As a preferred embodiment of the present invention, the ITO planar target blank is formed by pressing ITO powder with a purity of ≥4N.

[0010] As a preferred embodiment of the present invention, the specific process of degreasing is: heating to 400-800°C at a heating rate of 5-10°C / h, keeping warm for 5-12h, and then cooling to room temperature at a cooling rate of 80-120°C / h.

[0011] As a further preferred embodiment of the present invention, the specific process of degreasing is: heating to 500°C at a heating rate of 10°C / h, keeping the temperature for 10 hours, and then cooling to room temperature at a cooling rate of 100°C / h.

[0012] During the degreasing treatment of the target blank, no gas is required.

[0013] As a preferred embodiment of the present invention, the sealing structure is arranged in the following manner: a groove is provided on a sintering load-bearing plate in a sintering device, a sand layer with a depth greater than 25 mm is sprinkled in the groove, and then a sealing cover is embedded in the groove of the sintering load-bearing plate, so that the insertion depth of the sealing cover in the sand layer in the groove is 20 to 30 mm, so that the degreased ITO planar target blank is in a closed space.

[0014] The shape of the groove matches the shape of the sealing cover to form a sealing structure. If it is a sealing cover with a square groove, a connected square groove should be set on the sintered load-bearing plate, and the side length of the square groove is equal to or greater than the side length of the sealing cover. If it is a semicircular sealing cover, a circular groove should be set on the sintered load-bearing plate, and the diameter of the circular groove is equal to or greater than the diameter of the semicircular sealing cover.

[0015] As a preferred embodiment of the present invention, the sealing cover is an oxide of a high temperature resistant material; the sealing cover includes at least two connection ports, one of which is used to connect to an oxygen injection channel, and the other connection port is used to connect to an oxygen partial pressure test probe.

[0016] The oxygen partial pressure test probe can display the oxygen partial pressure value in the entire confined space in real time.

[0017] As a preferred embodiment of the present invention, the oxygen injection channel is a spiral gas injection pipeline with a spiral diameter of 30 to 100 mm, a number of spiral turns of 5 to 20, and a diameter of the injection pipeline opening of 5 to 20 mm.

[0018] As a further preferred embodiment of the present invention, the oxygen injection channel is a spiral gas injection pipeline with a spiral diameter of 30, a number of spiral turns of 10, and a diameter of the injection pipeline opening of 10 mm.

[0019] The spiral pipe is used to increase the movement distance of the gas, so that the normal temperature gas entering the furnace has enough time to be preheated in the pipe, so that the temperature of the gas entering the closed structure is consistent with the insulation temperature of the ITO flat target blank.

[0020] As a preferred embodiment of the present invention, the rate of introducing oxygen is 5 to 20 L / min; and the oxygen is high-purity oxygen.

[0021] The material of the sand layer is aluminum oxide with a purity greater than 4N, which is a high temperature resistant sand; the particle size of the sand layer is 50-200 meshes, and 100 meshes are more preferred.

[0022] As a preferred embodiment of the present invention, the depth of the sand layer is greater than 25 mm, more preferably 50 mm.

[0023] It is difficult to form a sealing structure when the sealing cover is in direct contact with the surface of the sintering load-bearing plate. A groove is set in the load-bearing plate and filled with a sand layer. The sealing cover is embedded in the sand layer to form a sealing structure. This structure not only has a good sealing effect, but is also stable and easy to install or disassemble, making the use or conversion of the sintering device more convenient.

[0024] As a preferred embodiment of the present invention, the heating rate of the sintering is 1-3°C / min, the sintering temperature is 1000-1700°C, the sintering time is 10-40h; the cooling rate after sintering is 1-5°C / min.

[0025] As a further preferred embodiment of the present invention, the heating rate of the sintering is 1.5°C / min, the sintering temperature is 1580°C, the sintering time is 20h; and the cooling rate after sintering is 5°C / min.

[0026] The present invention also provides an ITO planar target sintering device used in the above-mentioned ITO planar target sintering method, wherein the ITO planar target sintering device comprises a sealing structure; the sealing structure comprises an oxygen partial pressure test probe and an oxygen injection channel.

[0027] Conventional electrically heated sintering devices can be equipped with the sealing structure of the present invention through the method of the present invention to obtain the sintering device of the present invention. The method of modifying, installing or disassembling the sintering device of the present invention is simple, easy to use, low in cost and widely applicable.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] (1) In the sintering method of the present invention, the ITO planar target blank is sintered in a closed space suitable for its size. The temperature and gas distribution in the space are more uniform, which can improve the density of the target material and reduce the warping of the target material.

[0030] (2) The oxygen injection port of the sealing structure of the present invention adopts a spiral structure, so that the temperature of the gas entering the enclosed space is consistent with that in the enclosed space, reducing the influence of the sintering atmosphere on the sintering atmosphere due to the large deviation between the injected gas temperature and the sintering environment temperature, thereby avoiding the influence of the unstable sintering atmosphere on the sintering effect of the planar target.

[0031] (3) The sintering method of the present invention is carried out in a closed structure, which prevents oxygen from flowing out. After the oxygen partial pressure meets the conditions for suppressing the volatilization of the target material, there is no need to introduce oxygen, which greatly reduces the oxygen waste in the sintering process. The oxygen consumption required for the overall sintering process is extremely low. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is a schematic plan view of the sintering device of Examples 1-6.

[0033] Figure 2 It is a three-dimensional schematic diagram of the sintering device of Example 1-6.

[0034] The above drawings include the following figure marks: A oxygen partial pressure probe; B ITO flat target blank; C sand layer; D groove; E oxygen injection channel; F sealing cover; G sintering load-bearing plate. DETAILED DESCRIPTION

[0035] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below through specific comparative examples and embodiments.

[0036] The sintering devices of Examples 1-6 can be found in the attached Figure 1 and 2 Among them, conventional electrically heated sintering devices can be equipped with the sealing structure of the present invention through the method of the present invention to obtain the sintering device of the present invention, such as a common sintering device with a sintering temperature of ≤1800°C.

[0037] Example 1

[0038] (1) pressing ITO powder with a purity of ≥4N into an ITO flat target blank (B);

[0039] (2) Sprinkle a layer of high temperature resistant sand (alumina) at C of the sintering load-bearing plate (G) in the sintering device with a 50-mesh screen, and place B on the high temperature resistant sand; then heat to 500°C at a heating rate of 10°C / h, keep warm for 10h to complete the degreasing treatment of the target blank, and then cool to room temperature at 100°C / h;

[0040] (3) Before degreasing, a groove matching the size of the sealing cover has been opened on the sintering load-bearing plate, and the groove surrounds B. After the furnace is opened, 100-mesh alumina sand with a depth of 50 mm is sprinkled on the groove (D) around the sintering load-bearing plate, and the sealing cover (F) is embedded in the D position with an insertion depth of 25 mm, so that B is in a closed space; an oxygen injection pipe (E) with a spiral diameter of 30 mm, 10 spiral turns, and an injection port diameter of 10 mm is inserted into the right side of F, and an oxygen partial pressure probe (A) is inserted into the left side of F; the temperature is raised to 800°C at 2.5°C / min and kept warm. At the beginning of the heat preservation, oxygen is introduced at 20L / min. When the oxygen partial pressure test value reaches 30%, the heat preservation at 800°C is ended. Then the temperature is raised to 1580°C at 1.5°C / min, and after keeping warm for 20 hours, the temperature is lowered to room temperature at 5°C / min to obtain an ITO planar target.

[0041] The ITO planar target material has a warpage of 1.2 mm and a relative density of 98.7%.

[0042] Example 2

[0043] (1) pressing ITO powder with a purity of ≥4N into an ITO flat target blank (B);

[0044] (2) Sprinkle a layer of high temperature resistant sand (alumina) at C of the sintering load-bearing plate (G) in the sintering device with a 50-mesh screen, and place B on the high temperature resistant sand; then heat to 500°C at a heating rate of 10°C / h, keep warm for 10h to complete the degreasing treatment of the target blank, and then cool to room temperature at 100°C / h;

[0045] (3) After the furnace is opened, 100-mesh alumina sand with a depth of 50 mm is sprinkled on the grooves (D) around the sintering load-bearing plate, and the sealing cover (F) is embedded in the D position with an insertion depth of 25 mm, so that B is in a closed space; an oxygen injection pipe (E) with a spiral diameter of 30 mm, 10 spiral turns, and an injection port diameter of 10 mm is inserted into the right side of F, and an oxygen partial pressure probe (A) is inserted into the left side of F; the temperature is raised to 800°C at 2.5°C / min and kept warm, and oxygen is introduced at 15L / min at the beginning of the heat preservation. When the oxygen partial pressure test value reaches 50%, the heat preservation at 800°C is ended. Then the temperature is raised to 1580°C at 1.5°C / min, and after keeping warm for 20 hours, the temperature is lowered to room temperature at 5°C / min to obtain an ITO planar target.

[0046] The ITO planar target material has a warpage of 0.7 mm and a relative density of 99.4%.

[0047] Example 3

[0048] (1) pressing ITO powder with a purity of ≥4N into an ITO flat target blank (B);

[0049] (2) Sprinkle a layer of high temperature resistant sand (alumina) at C of the sintering load-bearing plate (G) in the sintering device with a 50-mesh screen, and place B on the high temperature resistant sand; then heat to 500°C at a heating rate of 10°C / h, keep warm for 10h to complete the degreasing treatment of the target blank, and then cool to room temperature at 100°C / h;

[0050] (3) Before degreasing, a groove matching the size of the sealing cover has been opened on the sintering load-bearing plate, and the groove surrounds B. After the furnace is opened, 100-mesh alumina sand with a depth of 50 mm is sprinkled on the groove (D) around the sintering load-bearing plate, and the sealing cover (F) is embedded in the D position with an insertion depth of 25 mm, so that B is in a closed space; an oxygen injection pipe (E) with a spiral diameter of 30 mm, 10 spiral turns, and an injection port diameter of 10 mm is inserted into the right side of F, and an oxygen partial pressure probe (A) is inserted into the left side of F; the temperature is raised to 800°C at 2.5°C / min and kept warm. At the beginning of the heat preservation, oxygen is introduced at 10L / min. When the oxygen partial pressure test value reaches 70%, the heat preservation at 800°C is ended. Then the temperature is raised to 1580°C at 1.5°C / min, and after keeping warm for 20 hours, the temperature is lowered to room temperature at 5°C / min to obtain an ITO planar target.

[0051] The ITO planar target material has a warpage of 0.2 mm and a relative density of 99.6%.

[0052] Example 4

[0053] (1) pressing ITO powder with a purity of ≥4N into an ITO flat target blank (B);

[0054] (2) Sprinkle a layer of high temperature resistant sand (alumina) at C of the sintering load-bearing plate (G) in the sintering device with a 50-mesh screen, and place B on the high temperature resistant sand; then heat to 500°C at a heating rate of 10°C / h, keep warm for 10h to complete the degreasing treatment of the target blank, and then cool to room temperature at 100°C / h;

[0055] (3) Before degreasing, a groove matching the size of the sealing cover has been opened on the sintering load-bearing plate, and the groove surrounds B. After the furnace is opened, 100-mesh alumina sand with a depth of 50 mm is sprinkled on the groove (D) around the sintering load-bearing plate, and the sealing cover (F) is embedded in the D position with an insertion depth of 25 mm, so that B is in a closed space; an oxygen injection pipe (E) with a spiral diameter of 30 mm, 10 spiral turns, and an injection port diameter of 10 mm is inserted into the right side of F, and an oxygen partial pressure probe (A) is inserted into the left side of F; the temperature is raised to 800°C at 2.5°C / min and kept warm. At the beginning of the heat preservation, oxygen is introduced at 5L / min. When the oxygen partial pressure test value reaches 90%, the heat preservation at 800°C is ended. Then the temperature is raised to 1580°C at 1.5°C / min, and after keeping warm for 20 hours, the temperature is lowered to room temperature at 5°C / min to obtain an ITO planar target.

[0056] The ITO planar target material has a warpage of 0.2 mm and a relative density of 99.8%.

[0057] Example 5

[0058] (1) pressing ITO powder with a purity of ≥4N into an ITO flat target blank (B);

[0059] (2) Sprinkle a layer of high temperature resistant sand (alumina) at C of the sintering load-bearing plate (G) in the sintering device with a 50-mesh screen, and place B on the high temperature resistant sand; then heat to 400°C at a heating rate of 5°C / h, keep warm for 5h, complete the degreasing treatment of the target blank, and then cool to room temperature at 8°C / h;

[0060] (3) Before degreasing, a groove matching the size of the sealing cover has been opened on the sintering load-bearing plate, and the groove surrounds B. After the furnace is opened, 50-mesh alumina sand with a depth of 25 mm is sprinkled on the groove (D) around the sintering load-bearing plate, and the sealing cover (F) is embedded in the D position with an insertion depth of 25 mm, so that B is in a closed space; an oxygen injection pipe (E) with a spiral diameter of 30 mm, 5 spiral turns, and an injection port diameter of 5 mm is inserted into the right side of F, and an oxygen partial pressure probe (A) is inserted into the left side of F; the temperature is raised to 600°C at 1°C / min and kept warm. At the beginning of the heat preservation, oxygen is introduced at 10L / min. When the oxygen partial pressure test value reaches 90%, the heat preservation at 600°C is ended. Then the temperature is raised to 1500°C at 1°C / min, and after keeping warm for 40 hours, the temperature is lowered to room temperature at 1°C / min to obtain an ITO planar target.

[0061] The ITO planar target material has a warpage of 0.2 mm and a relative density of 98.5%.

[0062] Example 6

[0063] (1) pressing ITO powder with a purity of ≥4N into an ITO flat target blank (B);

[0064] (2) Sprinkle a layer of high temperature resistant sand (alumina) at C of the sintering load-bearing plate (G) in the sintering device with a 200-mesh screen, and place B on the high temperature resistant sand; then heat to 800°C at a heating rate of 10°C / h, keep warm for 12h to complete the degreasing treatment of the target blank, and then cool to room temperature at 120°C / h;

[0065] (3) Before degreasing, a groove matching the size of the sealing cover has been opened on the sintering load-bearing plate, and the groove surrounds B. After the furnace is opened, 200-mesh alumina sand with a depth of 50 mm is sprinkled on the groove (D) around the sintering load-bearing plate, and the sealing cover (F) is embedded in the D position with an insertion depth of 25 mm, so that B is in a closed space; an oxygen injection pipe (E) with a spiral diameter of 100 mm, 20 spiral turns, and an injection port diameter of 20 mm is inserted into the right side of F, and an oxygen partial pressure probe (A) is inserted into the left side of F; the temperature is raised to 800°C at 3°C / min and kept warm. At the beginning of the heat preservation, oxygen is introduced at 5L / min. When the oxygen partial pressure test value reaches 90%, the heat preservation at 800°C is ended. Then the temperature is raised to 1700°C at 3°C / min, and after keeping warm for 10 hours, the temperature is lowered to room temperature at 5°C / min to obtain an ITO planar target.

[0066] The ITO planar target material has a warpage of 2.1 mm and a relative density of 99.2%.

[0067] Comparative Example 1

[0068] (1) Pressing ITO powder with a purity of ≥4N into an ITO planar target blank (the target blank is the same as that in Example 1);

[0069] (2) Sprinkle a layer of high temperature resistant sand (alumina) at C of the sintering load-bearing plate in the sintering device with a 50-mesh screen, and place B on the high temperature resistant sand; then heat to 500°C at a heating rate of 10°C / h, keep warm for 10h, complete the degreasing treatment of the target blank, and then cool to room temperature at 100°C / h;

[0070] (3) Raise the temperature to 800°C at 2.5°C / min and keep it warm. At the beginning of the heat preservation, introduce oxygen at 10L / min and keep the oxygen introduction. Then, raise the temperature to 1580°C at 1.5°C / min. After keeping it warm for 20 hours, cool it to room temperature at 5°C / min to obtain an ITO planar target.

[0071] The ITO planar target material of this comparative example has a warpage of 0.4 mm and a relative density of 99.6%.

[0072] Compared with Example 1, this comparative example is a conventional sintering method, and no sealing structure is set. Oxygen needs to be introduced all the time. The oxygen consumption throughout the process is large, about 26.8L liquid oxygen. Compared with Example 1, the oxygen consumption is only 0.3L liquid oxygen, which is an increase of 26.5L liquid oxygen. The method of the present invention can significantly reduce the oxygen consumption of sintering.

[0073] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A sintering method for an ITO planar target, It is characterized in that The steps include: (1) Placing the ITO planar target blank in a sintering device for degreasing; (2) A sealing structure is provided in the sintering device so that the degreased ITO planar target blank is placed in the sealing structure, wherein the sealing structure includes an oxygen partial pressure test probe and an oxygen injection channel; then the temperature is raised to 600-800°C at a heating rate of 1-5°C / min and the temperature is kept constant, during which oxygen is introduced through the oxygen injection channel, and when the oxygen partial pressure reaches 30%-90%, the introduction of oxygen is stopped and the temperature is kept constant; the temperature is then raised to the sintering temperature for sintering, and after the sintering is completed, the temperature is lowered to room temperature to obtain an ITO planar target; the sealing structure is provided in the following manner: a sintering support in the sintering device is provided; A groove is arranged on the weight plate, a sand layer with a depth greater than 25 mm is sprinkled in the groove, and then a sealing cover is embedded in the groove of the sintered load-bearing plate, so that the insertion depth of the sealing cover in the sand layer of the groove is 20-30 mm, so that the degreased ITO flat target blank is in a closed space; the sealing cover comprises at least two connecting ports, one of which is used to connect an oxygen injection channel, and the other is used to connect an oxygen partial pressure test probe; the oxygen injection channel is a spiral gas injection pipeline, the spiral diameter is 30-100 mm, the number of spiral turns is 5-20, and the diameter of the injection pipeline port is 5-20 mm.

2. The sintering method of the ITO planar target according to claim 1, It is characterized in that The specific process of degreasing is: heating to 400-800°C at a heating rate of 5-10°C / h, keeping the temperature for 5-12h, and then cooling to room temperature at a cooling rate of 80-120°C / h.

3. The sintering method of the ITO planar target according to claim 1, It is characterized in that The heating rate of the sintering is 1-3°C / min, the sintering temperature is 1000-1700°C, the sintering time is 10-40h; the cooling rate after sintering is 1-5°C / min.

4. The sintering method of the ITO planar target according to claim 1, It is characterized in that The rate of introducing oxygen is 5-20 L / min.

5. The sintering method of the ITO planar target according to claim 1, It is characterized in that The material of the sand layer is aluminum oxide with a purity greater than 4N; the particle size of the sand layer is 50-200 meshes.

6. A sintering device for ITO planar target, It is characterized in that The sintering device of the ITO planar target is used to execute the sintering method of the ITO planar target described in any one of claims 1 to 5, and the sintering device of the ITO planar target includes a sealing structure, and the sealing structure includes an oxygen partial pressure test probe and an oxygen injection channel. The sealing structure is arranged in the following manner: a groove is provided on a sintering load-bearing plate in the sintering device, a sand layer with a depth greater than 25 mm is sprinkled in the groove, and then a sealing cover is embedded in the groove of the sintering load-bearing plate, so that the insertion depth of the sealing cover in the sand layer in the groove is 20 to 30 mm, so that the degreased ITO planar target blank is in a confined space.