Ferritic stainless steel and method for producing ferritic stainless steel

By controlling the dispersion of the martensite phase and the work roll diameter in the cold rolling process, the problem of low drawing performance and wrinkle resistance in ferritic stainless steel is solved, and the ductility and wrinkle resistance of stainless steel are improved at low cost. , reducing the height of wrinkles and corrugations and enhancing the stability of the molding process.

CN115917029BActive Publication Date: 2024-10-29NIPPON STEEL STAINLESS STEEL CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202180044813.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-20
Publication Date
2024-10-29
Estimated Expiration
2041-10-20

AI Technical Summary

Technical Problem

It is difficult to improve the drawing performance and wrinkle resistance of ferritic stainless steel at the same time at low cost with existing technology, and expensive elements are added to existing methods or the wrinkle resistance cannot be fully improved.

Method used

By controlling the degree of dispersion of the martensite phase in ferritic stainless steel and the diameter of the work roll in the cold rolling process, the area ratio of the martensite phase after softening annealing is set to 5.0% or more and 30.0% or less, and In the cold rolling process, work rolls of more than 200mm are used for cold rolling to ensure that the total cold rolling rate reaches more than 50%.

Benefits of technology

It is possible to improve the deep drawing performance and anti-wrinkle performance of ferritic stainless steel at low cost, reduce the height of wrinkles and corrugations, enhance the surface quality and ease of forming processing, and avoid edge cracks and steel coil breakage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115917029B_ABST
    Figure CN115917029B_ABST
Patent Text Reader

Abstract

The present invention realizes ferritic stainless steel having excellent both deep drawing performance and wrinkle resistance at a lower cost than before. The ferritic stainless steel of the present invention has an average height of waviness curve elements in wrinkles formed on the surface of the ferritic stainless steel of 15 μm or less, an r value of 0.9 or more, and an area ratio of a martensite phase in a cross section cut along a plane parallel to the rolling direction and perpendicular to the width direction of 0% or more and less than 1.0%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to ferritic stainless steel and a method for producing ferritic stainless steel. Background Art

[0002] Ferritic stainless steel has excellent corrosion resistance and heat resistance, and is used in a variety of fields such as home appliances, cooking utensils, and construction. On the other hand, the ductility of ferritic stainless steel is inferior to that of austenitic stainless steel. In addition, ferritic stainless steel has the problem of wrinkles during forming, which affects the surface quality of the formed product and the grindability of the ferritic stainless steel after forming.

[0003] Here, wrinkles refer to surface defects generated on the surface of ferritic stainless steel, and specifically refer to strip-shaped or elongated strip-shaped undulations generated on the surface of ferritic stainless steel in a direction parallel to the processing direction. The "processing direction" is the direction in which the steel strip of ferritic stainless steel is stretched by forming. In addition, examples of forming processes that cause wrinkles include stamping, stretching, and drawing.

[0004] In order to improve the ductility of ferritic stainless steel, especially the deep drawing performance, it is generally known that reducing the C and N contents in the ferritic stainless steel is an effective method. On the other hand, it is also generally known that if the C and N contents in the ferritic stainless steel are reduced, the anti-wrinkling performance will be reduced. In view of these circumstances, it has been a long-standing issue to achieve ferritic stainless steel that is excellent in both deep drawing performance and anti-wrinkling performance.

[0005] In order to solve the above-mentioned problems, various studies have been carried out. For example, Patent Document 1 discloses a technology for manufacturing a ferritic stainless steel sheet with an improved r value and excellent anti-wrinkle performance by adding an amount of Ti that satisfies specified conditions and controlling the amount of precipitates. The r value (Lankford value) is a characteristic value representing the anisotropy of a general plate material, and becomes an indicator of the quality of the deep drawing performance of ferritic stainless steel. The larger the r value, the better the deep drawing performance of the ferritic stainless steel. In addition, for example, Patent Document 2 discloses a technology for manufacturing a ferritic stainless steel sheet with a large r value by cold rolling using a work roll with a specified roll diameter. The work roll is a component of a cold rolling mill that is in direct contact with the metal sheet to be rolled during cold rolling.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Laid-Open No. 10-130786

[0009] Patent Document 2: Japanese Patent Publication No. 59-107030 Summary of the invention

[0010] Problems to be solved by the invention

[0011] However, the technology disclosed in Patent Document 1 requires the addition of expensive element Ti, so the manufacturing cost of the ferritic stainless steel sheet becomes high. The technology disclosed in Patent Document 2 does not specify the manufacturing conditions and component composition for improving the anti-wrinkling performance, so the ferritic stainless steel sheet manufactured according to this technology cannot be said to have sufficient anti-wrinkling performance.

[0012] The technical solution of the present invention has been developed in view of the above-mentioned problems, and an object of the present invention is to realize a ferritic stainless steel having excellent both drawability and anti-wrinkling performance at a lower cost than before.

[0013] Technical solutions to solve problems

[0014] In order to solve the above-mentioned problems, the ferritic stainless steel according to the technical solution of the present invention is a ferritic stainless steel containing, in mass%, C: 0.12% or less, Si: 1.0% or less, Mn: 1.0% or less, Ni: 1.0% or less, Cr: 12.0% or more and 18.0% or less, N: 0.10% or less, and Al: 0.50% or less, with the remainder being Fe and inevitable impurities, wherein the average height of the waviness curve elements in the wrinkles formed on the surface of the ferritic stainless steel is 15 μm or less, the r value is 0.9 or more, and the ferritic stainless steel includes a martensitic phase whose area ratio in a cross section cut along a plane parallel to the rolling direction and perpendicular to the width direction is 0% or more and less than 1.0%.

[0015] In order to solve the above-mentioned problems, the method for producing ferritic stainless steel according to the technical solution of the present invention comprises: a hot rolling step of hot rolling a steel billet containing, by mass%, C: 0.12% or less, Si: 1.0% or less, Mn: 1.0% or less, Ni: 1.0% or less, Cr: 12.0% or more and 18.0% or less, N: 0.10% or less, and Al: 0.50% or less, with the remainder being Fe and unavoidable impurities, to produce a hot-rolled steel strip;

[0016] a softening annealing step of annealing the hot-rolled steel strip produced in the hot rolling step to soften it, thereby producing the hot-rolled annealed steel strip having an area ratio of 5.0% or more and 30.0% or less of a martensite phase in a cross section cut along a plane parallel to the rolling direction and perpendicular to the width direction of the hot-rolled annealed steel strip, and a remainder other than the martensite phase including a ferrite phase; and

[0017] a cold rolling step of cold rolling the hot-rolled annealed steel strip produced in the softening annealing step to produce a cold-rolled steel strip;

[0018] In the cold rolling process,

[0019] The total cold rolling ratio, which is the ratio of the difference between the thickness of the hot-rolled annealed steel strip and the thickness of the cold-rolled steel strip to the thickness of the hot-rolled annealed steel strip, is set to 60% or more.

[0020] For the hot rolled annealed steel strip,

[0021] (i) using a first working roll having a roll diameter of 200 mm or more, cold rolling is performed in such a manner that the cold rolling rate per pass is 15% or more and the cold rolling rate after all passes is 50% or more of the cold rolling rate, and then,

[0022] (ii) Cold rolling is further performed using a second work roll having a roll diameter of less than 200 mm.

[0023] Effects of the Invention

[0024] According to the technical aspects of the present invention, it is possible to realize ferritic stainless steel excellent in both drawability and anti-wrinkling performance at a lower cost than before. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a flowchart showing a method for producing ferritic stainless steel according to an embodiment of the present invention. DETAILED DESCRIPTION

[0026] The following is a detailed description of the embodiment of the present invention. In addition, in this specification, the content of each element relative to ferritic stainless steel (hereinafter referred to as "stainless steel") is referred to as content. In addition, unless otherwise specified, the expression "%" related to the content refers to "mass %". In addition, with respect to the numerical value X1 and the numerical value X2 (where X1 < X2), "X1-X2" means "more than X1 and less than X2".

[0027] [Mechanism of improving drawing performance and wrinkle resistance]

[0028] As a result of intensive research, the inventors have found an effective solution for achieving stainless steel with excellent both deep drawing performance and anti-wrinkling performance at a lower cost than before. Specifically, they have found that it is effective to appropriately set (i) the area ratio of the martensite phase after softening annealing, and (ii) the roll diameter of the work roll in cold rolling and the cold rolling conditions. The relevant contents are described below.

[0029] <Improvement of ductility and wrinkle resistance>

[0030] First, the research results of the inventors and others related to the scheme (i) are described. As a common knowledge, it is known that the dispersion of the martensitic phase occurs by performing a softening annealing on a stainless steel strip after hot rolling (the details will be described later). Hereinafter, the stainless steel strip will be referred to as a "stainless steel strip". "Dispersion of the martensitic phase" means that the austenite phase in the stainless steel strip is transformed into a martensitic phase, and the martensitic phase is dispersed in the ferrite phase in the stainless steel strip. The dispersion of the martensitic phase has the effect of dividing the crystal clusters (textures of similar crystal orientations) of the ferrite phase during cold rolling after the softening annealing.

[0031] Here, wrinkling is a phenomenon caused by the continuous existence of crystal clusters in stainless steel along the rolling direction, so the dispersion of the martensite phase becomes effective in improving the wrinkle resistance. The "rolling direction" is the direction in which the stainless steel strip passes through the rolling device when the stainless steel strip is rolled.

[0032] However, if the martensite phase is dispersed excessively, the amount of the martensite phase in the stainless steel strip after the softening annealing will increase excessively. The martensite phase is a hard and high-strength structure, and the ferrite phase is a soft and ductile structure, so the ductility of the stainless steel cannot be improved. In addition, when the stainless steel strip after the softening annealing is cold rolled, it will cause edge cracks and steel coil (steel strip) breakage.

[0033] On the other hand, if the dispersion of the martensite phase is small, the division of the martensite phase into ferrite phase crystals during cold rolling after softening annealing will become insufficient, and the anti-wrinkling performance of the stainless steel cannot be improved.

[0034] Based on these circumstances, as a result of intensive research, the present inventors have come to the following conclusion: With regard to stainless steel, in order to maintain the strength at the original level and improve the ductility and wrinkle resistance, it is effective to appropriately disperse the martensite phase. Specifically, the present inventors have found that dispersing the martensite phase is effective in ensuring that the area ratio of the martensite phase in the stainless steel strip after softening annealing is 5.0 to 30.0%.

[0035] The "area ratio of the martensite phase after softening annealing" refers to the ratio of the total area of ​​the martensite phase region contained in the cut section relative to the area of ​​the cut section in the stainless steel strip after softening annealing. The cut section is a cross section formed when the stainless steel strip after softening annealing is cut along a plane parallel to the rolling direction and perpendicular to the width direction of the stainless steel strip. Hereinafter, the area ratio of the martensite phase after softening annealing is referred to as the "first martensite area ratio".

[0036] The first martensite area ratio can be calculated using, for example, EBSD (electron backscattering diffraction) crystal orientation analysis. Specifically, first, an EBSD pattern of the measurement surface of the softened annealed stainless steel strip is obtained using an EBSD detector mounted on a scanning electron microscope (SEM). Regarding the acquisition of the EBSD pattern, the acquisition conditions can be set as follows, for example.

[0037] · Measurement surface: L cross-section (cutting cross-section: the cross-section formed by cutting the softened annealed stainless steel strip with a plane parallel to the rolling direction and perpendicular to the width direction of the softened annealed stainless steel strip)

[0038] · Magnification: 100 - 800 times

[0039] · Measurement area: 100 - 1000 μm square

[0040] · Measurement pitch (step size): 0.3 - 0.8 μm

[0041] Next, based on the obtained EBSD pattern, an IQ (Image Quality) image is generated using QIM (Orientation Imaging Microscopy) analysis software. The IQ image is an image that represents each structure formed on the measurement surface of the hot-rolled annealed steel strip by the level of visibility. Compared with the ferrite phase, the martensite phase has a more complex internal structure and lower visibility. Therefore, the martensite phase region in the measurement surface appears relatively dim in the IQ image. On the other hand, compared with the martensite phase, the ferrite phase has a simpler internal structure and higher visibility. Therefore, the ferrite phase region in the measurement surface appears relatively bright in the IQ image. By binarizing this IQ image and dividing the total area of the martensite phase region by the area of the measurement surface, the first martensite area ratio can be calculated.

[0042] The inventors have found that by setting the first martensite area ratio to 5.0% or more, the ripple height of the wrinkles formed on the surface of the stainless steel is lower than before, the surface properties of the stainless steel are improved, and the forming process becomes easier. In addition, the inventors have found that by setting the first martensite area ratio to 30.0% or less, the ductility of the softened annealed stainless steel strip will not decrease, and cold ductility defects such as edge cracking and coil breakage are not likely to occur during the cold rolling process.

[0043] <Improvement of r value>

[0044] If only the solution (i) is adopted, although the ductility of the stainless steel will be improved, it cannot be said that the improvement in the drawing performance is sufficient. In response to this, the present inventors further conducted research and found that the solution (ii) is effective in improving the drawing performance of stainless steel. The following is an explanation of the research results of the present inventors related to (ii). As a general knowledge, it is known that regarding the r value as an indicator of the quality of the drawing performance in stainless steel, the more crystal orientations with Miller index {111} (hereinafter referred to as "{111} crystal orientation") generated in the stainless steel, the larger the r value. The {111} crystal orientation has the following tendency: it is generated in the area where rolling strain occurs; therefore, in stainless steel, it is easy to be generated at the grain boundary where the rolling strain is concentrated.

[0045] Here, if the stainless steel strip after the soft annealing is cold rolled using a work roll having a roll diameter of 50 to 100 mm, which is generally used in cold rolling, there is a tendency that the concentration of rolling strain is limited to the end portion in the thickness direction of the stainless steel strip after cold rolling. In other words, there is a tendency that the concentration of rolling strain is difficult to occur in the center portion in the thickness direction of the stainless steel strip after cold rolling, and it is difficult to generate a grain boundary. Hereinafter, the center portion in the thickness direction of the stainless steel strip is referred to as the "thickness center portion", and the end portion in the thickness direction is referred to as the "thickness surface portion". In order to increase the r value, it is necessary to generate more {111} crystal orientation in all parts from the thickness surface portion to the thickness center portion. Therefore, if the general work roll is used, it is not possible to generate more {111} crystal orientation in the thickness center portion, and it is difficult to increase the r value of the stainless steel.

[0046] Based on these circumstances, the inventors of the present invention considered that if the roll diameter is set larger than that of the general work roll, rolling strain may be easily concentrated in the center of the plate thickness, and grain boundaries may be easily generated, so that more {111} crystal orientations can be generated. This consideration is based on the fact that if the distance between the surface of the stainless steel strip and the rotation axis is the same in the general work roll and the work roll with a larger roll diameter, the work roll with a larger roll diameter can roll to a portion closer to the center of the plate thickness.

[0047] As a result of in-depth research based on the above considerations, it was determined that if the roll diameter of the work roll is set to 200 mm or more, it is possible to generate the desired amount of {111} crystal orientation in all parts from the surface layer part to the center part of the plate thickness. However, as a result of further research, it was determined that even if the roll diameter of the work roll is set to 200 mm or more, the cold rolling rate per pass in cold rolling is low, and if the cold rolling rate of cold rolling using the work roll is low, it is difficult to generate the desired amount of {111} crystal orientation in the center part of the plate thickness. In addition, the cold rolling rate per pass refers to the ratio of the difference between the thickness of the stainless steel strip in the previous pass and the thickness of the stainless steel strip after passing through one pass to the thickness of the stainless steel strip in the previous pass for any pass.

[0048] In this regard, the inventors of the present invention have conducted further research. As a result, the following insights were obtained: setting the roll diameter of the working roll to be greater than 200 mm, setting the cold rolling rate of each pass to be greater than 15%, and setting the cold rolling rate after all passes to be greater than 50% of the total cold rolling rate are effective in improving the r value of stainless steel. Here, the total cold rolling rate refers to the ratio of the difference between the thickness of the hot-rolled annealed steel strip before cold rolling and the thickness of the cold-rolled steel strip to the thickness of the hot-rolled annealed steel strip. The cold-rolled steel strip used as the basis for calculating the total cold rolling rate refers to the steel strip after all the treatments in the cold rolling are completed (in this embodiment, after the first cold rolling and the second cold rolling described later are completed). The cold rolling rate after all passes will be described later.

[0049] That is, the following conclusion was reached: by setting the roll diameter of the working roll to be greater than 200 mm, setting the cold rolling rate of each pass to be greater than 15%, and setting the cold rolling rate after all passes to be greater than 50% of the total cold rolling rate, the desired amount of {111} crystal orientation can be generated in all parts from the surface part to the center part of the plate thickness.

[0050] In the following description, work rolls with a roll diameter of 200 mm or more are called "large-diameter rolls", and work rolls with a roll diameter of less than 200 mm are called "small-diameter rolls". Based on these definitions, work rolls with a roll diameter of 50 to 100 mm generally used in cold rolling belong to "small-diameter rolls".

[0051] <Conclusion>

[0052] If stainless steel is manufactured based on the above-mentioned solutions (i) and (ii), it is no longer necessary to add expensive elements such as Ti as in the previous manufacturing method in order to improve both the deep drawing performance and the anti-wrinkle performance. In addition, it is not necessary to set up special manufacturing equipment for improving both the deep drawing performance and the anti-wrinkle performance. Therefore, the above-mentioned solutions (i) and (ii) are effective in achieving stainless steel with excellent deep drawing performance and anti-wrinkle performance at a lower cost than before.

[0053] [Mechanism of improvement of corrosion resistance and processability]

[0054] As a result of further studies, the present inventors have found that by eliminating the martensite phase in the cold-rolled steel strip obtained based on each of the above-mentioned solutions (i) and (ii), stainless steel having excellent corrosion resistance and workability can be achieved at a lower cost than before.

[0055] Specifically, in the finished annealing after cold rolling, the cold-rolled steel strip is heated to a temperature above 800°C and below Ac1 at a heating rate of less than 50°C / s. Ac1 is the benchmark for the start temperature of the formation of the austenite phase. Through this heating treatment, the martensite phase begins to disappear from the moment the cold-rolled steel strip reaches a certain temperature (about 700°C). Next, the heated cold-rolled steel strip is heat-treated for more than 5 seconds in a temperature range of more than 800°C and less than Ac1, so that the martensite phase in the cold-rolled steel strip disappears approximately. Subsequently, the heat-treated cold-rolled steel strip is cooled at a cooling rate of less than 50°C / s, with the goal of making the martensite phase in the cold-rolled steel strip disappear.

[0056] In this specification, "disappearance of martensitic phase" means that the area ratio of martensitic phase contained in the stainless steel as the final product is substantially 0%, that is, the martensitic phase in the stainless steel as the final product is substantially completely disappeared. "Area ratio of martensitic phase contained in the stainless steel as the final product" means the ratio of the total area of ​​the martensitic phase region contained in the cross section of the stainless steel as the final product to the area of ​​the cross section. The cross section is a cross section formed when the stainless steel as the final product is cut in a plane parallel to the rolling direction and perpendicular to the width direction of the stainless steel.

[0057] However, regarding the concept of "disappearance of the martensite phase" in this specification, the goal is the complete disappearance of the martensite phase (area ratio 0%), and it is allowed that as a result of the finish annealing, a martensite phase with an area ratio of less than 1.0% remains in the stainless steel as the final product. If the area ratio of the remaining martensite phase is less than 1.0%, the corrosion resistance and workability of the stainless steel as the final product are excellent. Hereinafter, the area ratio of the martensite phase contained in the stainless steel as the final product is referred to as the "second martensite area ratio".

[0058] The inventors have found that by performing the above-mentioned finish annealing on cold-rolled steel strips, recrystallization of the ferrite phase as the parent phase can be completed, and the martensite phase (first martensite area ratio of 5.0 to 30.0%) expected to be generated during softening annealing also disappears. Recrystallization means the generation of new grains without dislocations in cold-rolled steel strips. Dislocations are an example of lattice defects generated inside the crystal. Also, the inventors have found that by performing the above-mentioned finish annealing on cold-rolled steel strips, the generation of new martensite phases in the cold-rolled steel strips can be prevented. The above series of techniques from softening annealing to finish annealing are different from the manufacturing methods of general stainless steels that aim to actively disappear the martensite phase from the moment of performing softening annealing.

[0059] 〔Composition〕

[0060] The stainless steel according to the embodiment of the present invention contains, by mass%, C: 0.12% or less, Si: 1.0% or less, Mn: 1.0% or less, Ni: 1.0% or less, Cr: 12.0 to 18.0%, N: 0.10% or less, Al: 0.50% or less, Mo: 0.50% or less, Cu: 1.0% or less, O: 0.01% or less, V: 0.15% or less, B: 0.10% or less, Ti: 0.50% or less, Co: 0.01 to 0.50%, Zr: 0.01 to 0.10%, Nb: 0.01 to 0.10%, Mg: 0.0005 to 0.003%, Ca: 0.0003 to 0.003%, Y: 0.01% to 0.20%, rare earth metals (REM) other than Y: in total 0.01 to 0.10%, Sn: 0.001 to 0.50%, Sb: 0.001 to 0.50%, Pb: 0.01 to 0.10%, and W: 0.01 to 0.50%. In the following description, the stainless steel according to the embodiment of the present invention will be simply referred to as "this stainless steel".

[0061] The remainder of this stainless steel is composed of Fe and inevitable impurities. In addition, Mo, Cu, O, V, B, Ti, Co, Zr, Nb, Mg, Ca, Y, REM, Sn, Sb, Pb, and W are not essential elements of this stainless steel respectively. These elements are optional elements, and at least one or more of these elements may be contained as needed. Hereinafter, each element contained in this stainless steel will be described.

[0062] <C: 0.12% or less>

[0063] C is an important element that forms carbides with Cr and generates an interface that becomes a dislocation generation source during the deformation of this stainless steel. However, if C is added in excess, martensite phases will be generated excessively, resulting in a decrease in the ductility of this stainless steel. Therefore, the content rate of C is set to 0.12% or less.

[0064] <Si: 1.0% or less>

[0065] Si has the effect of being a deoxidizer in the smelting stage. However, if Si is added in excess, this stainless steel will be hardened and its ductility will decrease. Therefore, the content rate of Si is set to 1.0% or less.

[0066] <Mn: 1.0% or less>

[0067] Mn has the effect of being a deoxidizer. However, if Mn is added in excess, the amount of MnS generated will increase and the corrosion resistance of this stainless steel will decrease. Therefore, the content rate of Mn is set to 1.0% or less.

[0068] <Ni: 1.0% or less>

[0069] Ni is an austenite-forming element and is an element effective for controlling the area ratio of the first martensite and the strength of this stainless steel. However, if Ni is added in excess, the austenite phase will be overly stabilized, resulting in a decrease in the ductility of this stainless steel and an increase in the raw material cost of this stainless steel at the same time. Therefore, the content rate of Ni is set to 1.0% or less. In addition, in the following description, the steel strip of this stainless steel after softening annealing will be referred to as "hot-rolled annealed steel strip". The steel strip of this stainless steel after softening annealing is an example of the hot-rolled annealed steel strip related to the present invention.

[0070] <Cr: 12.0 - 18.0%>

[0071] Cr is necessary to form a passive film on the surface of the steel strip of this stainless steel after cold rolling and improve the corrosion resistance. However, if Cr is added in excess, the ductility of this stainless steel will decrease. Therefore, the content rate of Cr is set to 12.0 - 18.0%. In addition, in the following description, the steel strip of this stainless steel after cold rolling will be referred to as "cold-rolled steel strip". The steel strip of this stainless steel after cold rolling is an example of the cold-rolled steel strip related to the present invention.

[0072] <N: 0.10% or less>

[0073] N is an important element that forms nitrides with Cr and generates an interface that becomes a source of dislocations when this stainless steel is deformed. However, if N is added in excess, the martensite phase will be overly generated, resulting in a decrease in the ductility of this stainless steel. Therefore, the content rate of N is set to 0.10% or less.

[0074] <Al: 0.50% or less>

[0075] Al is an element effective for deoxidation and can also reduce A that has an adverse effect on stamping workability 2Inclusions of this type. However, if the addition of Al is excessive, the surface defects of this stainless steel increase. Therefore, the Al content is set to 0.50% or less.

[0076] <Mo: Preferably 0.5% or less>

[0077] Mo is an element effective in improving corrosion resistance. However, if the addition of Mo is excessive, the raw material cost of this stainless steel increases. Therefore, the Mo content is preferably set to 0.50% or less.

[0078] <Cu: Preferably 1.0% or less>

[0079] Cu is an element effective in improving corrosion resistance. The Cu content is preferably set to 1.0% or less.

[0080] <O: Preferably 0.01% or less>

[0081] O generates non-metallic inclusions, thereby reducing the impact value and fatigue life of this stainless steel. Therefore, the O content is preferably set to 0.01% or less.

[0082] <V: Preferably 0.15% or less>

[0083] V is an element effective in improving hardness and strength. However, if the addition of V is excessive, the raw material cost of this stainless steel increases. Therefore, the V content is preferably set to 0.15% or less.

[0084] <B: Preferably 0.10% or less>

[0085] B is an element effective in improving toughness. However, this effect saturates when it exceeds 0.10%. Therefore, the B content is preferably set to 0.10% or less.

[0086] <Ti: Preferably 0.50% or less>

[0087] Ti is an element that forms carbonitrides, inhibits the grain boundary precipitation of Cr carbonitrides during heat treatment, and improves the corrosion resistance of this stainless steel. Also, by fixing the dissolved C and dissolved N in this stainless steel as carbonitrides, the contents of dissolved C and dissolved N can be reduced, and the r value of this stainless steel can be increased. Furthermore, by fixing the dissolved C and dissolved N in this stainless steel as carbonitrides, the ductility of this stainless steel can be improved while reducing the tensile strain. Tensile strain is the minute unevenness formed on the surface of stainless steel due to the several percent yield elongation generated during the stamping process of stainless steel.

[0088] However, since Ti is an expensive element, if the addition of Ti is excessive, the raw material cost of this stainless steel increases. Therefore, the Ti content is preferably set to 0.50% or less.

[0089] <Co: Preferably 0.01 to 0.50%>

[0090] Co is an element effective in improving corrosion resistance and heat resistance. However, if the addition of Co is excessive, the raw material cost of this stainless steel increases. Therefore, the content rate of Co is preferably set to 0.01 to 0.50%.

[0091] <Zr: Preferably 0.01 to 0.10%>

[0092] Zr is an element effective in denitrification, deoxidation, and desulfurization. However, if the addition of Zr is excessive, the raw material cost of this stainless steel increases. Therefore, the content rate of Zr is preferably set to 0.01 to 0.10%.

[0093] <Nb: Preferably 0.01 to 0.10%>

[0094] Similar to Ti, Nb can reduce the content of dissolved C and dissolved N and increase the r value of this stainless steel by fixing the dissolved C and dissolved N in this stainless steel as carbonitrides. Also, by fixing the dissolved C and dissolved N in this stainless steel as carbonitrides, the ductility of this stainless steel can be improved, and at the same time, tensile strain can be reduced. However, since Nb is an expensive element, if the addition of Nb is excessive, the raw material cost of this stainless steel increases. Therefore, the content rate of Nb is preferably set to 0.01 to 0.10%.

[0095] <Mg: Preferably 0.0005 to 0.003%>

[0096] Mg forms Mg oxide together with Al in the molten steel and acts as a deoxidizer. However, if the addition of Mg is excessive, the toughness of this stainless steel decreases, and furthermore, the manufacturability decreases. Therefore, the content rate of Mg is preferably set to 0.0005 to 0.003%, and more preferably set to 0.002% or less.

[0097] <Ca: Preferably 0.0003 to 0.003%>

[0098] Ca is an element effective in degassing. The content rate of Ca is preferably set to 0.0003 to 0.003%.

[0099] <Y: Preferably 0.01 to 0.20%>

[0100] Y is an element effective in improving hot workability and oxidation resistance. However, these effects saturate when exceeding 0.20%. Therefore, the content rate of Y is preferably set to 0.01 to 0.20%.

[0101] <REM: Preferably the total is 0.01 to 0.10%>

[0102] Similar to Y, REMs (Rare Earth Metals) such as Sc and La are effective in improving hot workability and oxidation resistance. However, these effects saturate when exceeding 0.10%. Therefore, the total content of REMs is preferably set to 0.01 - 0.10%.

[0103] <Sn: Preferably 0.001 - 0.50%>

[0104] Sn is an element effective in improving corrosion resistance. However, if the addition of Sn is excessive, hot workability and flexibility decrease. Therefore, the content of Sn is preferably set to 0.001 - 0.50%.

[0105] <Sb: Preferably 0.001 - 0.50%>

[0106] Sb is effective in improving workability by promoting the generation of deformation bands during rolling. However, if the addition of Sb is excessive, this effect saturates and workability decreases according to the amount of excessive Sb added. Therefore, the content of Sb is preferably set to 0.001 - 0.50%, more preferably 0.20% or less.

[0107] <Pb: Preferably 0.01 - 0.10%>

[0108] Pb is an element effective in improving machinability. The content of Pb is preferably set to 0.01 - 0.10%.

[0109] <W: Preferably 0.01 - 0.50%>

[0110] W is an element effective in improving high-temperature strength. However, if the addition of W is excessive, the raw material cost of this stainless steel increases. Therefore, the content of W is preferably set to 0.01 - 0.50%.

[0111] <Others>

[0112] In this stainless steel, the remainder other than the above components is Fe and inevitable impurities. Inevitable impurities are impurities mixed in from raw materials and manufacturing processes and are mixed within the range that does not affect the characteristics of the above components.

[0113] 〔Ripple height of wrinkles〕

[0114] The ripple height of the wrinkles formed on the surface of this stainless steel is 15 μm or less. In this specification, "the ripple height of the wrinkles formed on the surface of this stainless steel (hereinafter simply referred to as "the ripple height of this stainless steel")" refers to the ripple height of the wrinkles measured by the method shown below.

[0115] First, a JIS No. 5 tensile test piece specified in JIS Z 2201 (hereinafter referred to as the "first tensile test piece") is collected from the final product of the stainless steel. Next, an Instron tensile tester is used, the gauge length is set to 50 mm, and the first tensile test piece is stretched in a direction parallel to the rolling direction as the tensile direction. Then, a tensile strain of 16% is given to the first tensile test piece through the tensile test. Subsequently, a surface roughness measuring instrument is used to measure the corrugation height of 18 mm in the direction orthogonal to the rolling direction (in other words, the width direction of the first tensile test piece) in the portion between the calibration points of the first tensile test piece.

[0116] The corrugation height is the average height of the corrugation curve element measured according to the surface property measurement specified in JIS B 0601:2001, etc. In the present embodiment, the average height of the corrugation curve element of the first tensile test piece is measured according to the surface property measurement specified in JIS B 0601:2001. The average height of the corrugation curve element measured by this method becomes the corrugation height of the present stainless steel.

[0117] When the corrugation height of the wrinkles formed on the surface of conventional stainless steel was measured by the above method, the corrugation height was 20 to 50 μm, which was higher than that of the present stainless steel. It can be concluded that the anti-wrinkle performance of the present stainless steel is improved over that of conventional stainless steel.

[0118] 〔r value〕

[0119] The r value of the present stainless steel is 0.9 or more. In this specification, the "r value of the present stainless steel" means the r value calculated by the following method.

[0120] First, a JIS 13B tensile test piece specified in JIS Z 2201 is collected from the final product of the stainless steel. Specifically, a second tensile test piece whose direction parallel to the rolling direction is the tensile direction, a third tensile test piece whose direction forming a 45° angle with the rolling direction is the tensile direction, and a fourth tensile test piece whose direction orthogonal to the rolling direction is the tensile direction are collected from the final product. Next, for the second to fourth tensile test pieces, the gauge length is set to 20 mm, and the tensile test is performed using an Instron tensile tester. Then, through this tensile test, a tensile strain of 14.4% is given to the second to fourth tensile test pieces, respectively.

[0121] Next, the r value of each of the second to fourth tensile test pieces was calculated using the following formula (1).

[0122] r=ln(W / W1) / ln(t / t1)…(1)

[0123] Here, W is the width before the tensile test, W1 is the width after the tensile test, t is the thickness before the tensile test, and t1 is the thickness after the tensile test. "Width" is the width of the portion between the calibration points of each of the second to fourth tensile test pieces. "Thickness" is the thickness of the portion between the calibration points of each of the second to fourth tensile test pieces.

[0124] Next, the average r value obtained by averaging the r values ​​of the second to fourth tensile test pieces was calculated using the following formula (2). This average r value became the r value of the present stainless steel.

[0125] Average r value = (r0+2r45+r90) / 4…(2)

[0126] Here, r0 is the r value of the second tensile test piece, r45 is the r value of the third tensile test piece, and r90 is the r value of the fourth tensile test piece.

[0127] When the r value of conventional stainless steel is calculated by the above method, the r value is 0.6 to 0.8, which is smaller than the r value of the present stainless steel. It can be concluded that the deep drawing performance of the present stainless steel is improved compared with conventional stainless steel.

[0128] [Area ratio of second martensite]

[0129] The second martensite area ratio of the present stainless steel is 0% or more and less than 1.0%. From the viewpoint of improving the corrosion resistance and processability of the present stainless steel, the second martensite area ratio is preferably 0%. However, if the second martensite area ratio is less than 1.0%, even if the area ratio is higher than 0%, the present stainless steel not only has excellent wrinkle resistance and deep drawing performance, but also has excellent corrosion resistance and processability. The second martensite area ratio can be calculated using EBSD crystal orientation analysis in the same way as the first martensite area ratio.

[0130] 〔Indicator value〕

[0131] The index value of the present stainless steel represented by the following formula (3) is 15 to 50. This index value is an index indicating the maximum amount of austenite phase generated by annealing. In the following formula (3), each element symbol indicates the mass % concentration of the element.

[0132] (Indicator value) = 420C-11.5Si+7Mn+23Ni-11.5Cr-12Mo+9Cu-49Ti-52Al+470N+189…(3)

[0133] The austenite phase generated during annealing can be transformed into the martensite phase during the cooling process. Therefore, by adjusting the mass % concentration of each element in the formula (3) so that the index value reaches 15 to 50, the amount of the martensite phase generated during the cooling process can be properly managed. "Proper management" specifically means that the maximum amount of austenite phase generated by annealing is controlled so that the amount of the martensite phase generated during the cooling process reaches an amount that can achieve both improved drawing performance and improved wrinkle resistance. In addition, by using an index value of 15 to 50, the amount of the martensite phase is properly managed, so it is easy to manage the first martensite area ratio to 5.0 to 30.0%.

[0134] [Manufacturing method of stainless steel]

[0135] use Figure 1 The method for manufacturing the stainless steel according to the embodiment of the present invention is described. Figure 1 As shown in FIG. 1 , the stainless steel is manufactured through the steps of melting step S1, hot rolling step S2, softening annealing step S3, cold rolling step S4 and annealing step S5. Each step will be described below, but the manufacturing method of the stainless steel is not limited to Figure 1 The method shown.

[0136] <Melt-making process S1 and hot rolling process S2>

[0137] In order to manufacture the present stainless steel, first, in the smelting step S1, the stainless steel containing the above-mentioned components is smelted to manufacture a steel slab. In the smelting step S1, a general smelting device for stainless steel can be used, and general smelting conditions can be set. Next, in the hot rolling step S2, the steel slab manufactured in the smelting step S1 is hot rolled to manufacture a hot-rolled steel strip. This hot-rolled steel strip is an example of the hot-rolled steel strip involved in the present invention. In the hot rolling step S2, a general hot rolling device and hot rolling conditions for stainless steel can be used.

[0138] <Softening Annealing Step S3>

[0139] Next, in the softening annealing step S3, the hot-rolled steel strip manufactured in the hot rolling step S2 is subjected to softening annealing to manufacture a hot-rolled annealed steel strip. Softening annealing is a heat treatment for annealing the hot-rolled steel strip by setting the maximum temperature during the soaking process to Ac1 or more in order to soften the hot-rolled steel strip. By performing softening annealing to soften the hot-rolled steel strip, it becomes easy to adjust the thickness of the hot-rolled annealed steel strip in the subsequent cold rolling step S4.

[0140] Generally, when the temperature during the soaking process in the softening annealing exceeds Ac1, the amount of austenite phase in the steel strip begins to increase. Then, if the temperature of the softening annealing is further increased, the amount of austenite phase in the steel strip increases to a peak amount and then decreases. The austenite phase can be transformed into the martensite phase during the cooling process in the softening annealing. Therefore, the first martensite area ratio is affected by the austenite phase increased by the softening annealing. Therefore, in order to make the first martensite area ratio 5.0-30.0%, it is necessary to set the maximum annealing temperature to above Ac1 and below the temperature at which the amount of austenite phase does not increase excessively. The maximum annealing temperature is the highest temperature during the soaking process in the softening annealing.

[0141] However, Ac1 is the standard temperature in the regression equation, which is not consistent with the actual temperature at which the austenite phase begins to form. As a result of in-depth research, the inventors found that when Ac1 is less than 921, the first martensite area ratio can be set to 5.0 to 30.0% by setting the maximum annealing temperature to 0.76×Ac1+201°C or more and 1.10×Ac1-56°C or less.

[0142] On the other hand, when Ac1 is 921 or more, the peak amount of the austenite phase itself is small, so even if the entire peak amount is transformed from the austenite phase to the martensite phase, the first martensite area ratio can be set to 5.0 to 30.0%. Therefore, when Ac1 is 921 or more, it is not necessary to set the upper limit of the maximum annealing temperature to 1.10×Ac1-56°C. Here, since softening annealing at excessively high temperatures will cause coarsening of grains in the hot-rolled annealed steel strip and deterioration of properties such as surface roughness during processing, it is decided to set the upper limit of the maximum annealing temperature to 1050°C.

[0143] Specifically, the maximum annealing temperature is set as follows. First, based on the composition of the steel slab, Ac1 represented by the following formula (4) is calculated. In the following formula (4), each element symbol represents the mass % concentration of the element. This Ac1 only needs to be calculated in advance.

[0144] Ac1=35×(Cr+1.72Mo+2.09Si+4.86Nb+8.29V+1.77Ti+21.4Al+40B-7.14C-8.0N-3.24Ni-1.89Mn-0.51Cu)+310…(4)

[0145] Then, when Ac1 calculated by the formula (4) is less than 921, the maximum annealing temperature is set to be 0.76×Ac1+201°C or more and 1.10×Ac1-56°C or less. On the other hand, when Ac1 calculated by the formula (4) is 921 or more, the maximum annealing temperature is set to be 0.76×Ac1+201°C or more and 1050°C or less.

[0146] The heating rate of the heating process in the softening annealing is preferably set to be above 10°C / sec. If the heating rate is above 10°C / sec, the heating time in the heating process can be shortened to a practical and meaningful level, so the total time required for the manufacture of the present stainless steel can also be shortened to a practical and meaningful level. Therefore, the productivity of the present stainless steel can be improved. In addition, the soaking time of the soaking process in the softening annealing is preferably set to be above 5 seconds. If the soaking time is above 5 seconds, the austenite phase can be reliably generated during the soaking process. Since the austenite phase will transform into the martensite phase during the cooling process after the soaking process, it will be easier to manage the first martensite area ratio to 5.0 to 30.0% by setting the soaking time to be above 5 seconds.

[0147] Furthermore, the cooling rate of the cooling process in the softening annealing is set to be 5.0°C / sec or more. If the cooling rate is less than 5.0°C / sec, the cooling time in the cooling process will be extended beyond necessity, and the austenite phase will transform into a stable ferrite phase. Therefore, the first martensite area ratio will be reduced to less than 5.0%, and the wrinkle resistance of the present stainless steel will be reduced to less than that of the conventional stainless steel. Accordingly, in order to ensure the wrinkle resistance of the present stainless steel well, the cooling rate is set to be 5.0°C / sec or more.

[0148] <Cold rolling process S4>

[0149] Next, in the cold rolling step S4, the hot-rolled annealed steel strip produced in the softening annealing step S3 is cold rolled to produce a cold-rolled steel strip. As the cold rolling conditions, the total cold rolling rate after the cold rolling step S4 is set to 60% or more.

[0150] Regarding the cold rolling in the cold rolling process S4, first, the first cold rolling is performed to pass the hot-rolled annealed steel strip through a large-diameter working roll with a roll diameter of 200 mm or more. The large-diameter working roll with a roll diameter of 200 mm or more is an example of the first working roll involved in the present invention. As the cold rolling conditions of the first cold rolling, the cold rolling rate of each pass is set to be 15% or more, and the cold rolling rate after the first cold rolling is completed (after all passes in the first cold rolling are completed) is set to be 50% or more of the total cold rolling rate. The cold rolling rate after the first cold rolling is completed (after all passes in the first cold rolling are completed) refers to the ratio of the difference between the thickness of the hot-rolled annealed steel strip before the first cold rolling and the thickness of the steel strip after all passes are completed to the thickness of the hot-rolled annealed steel strip.

[0151] After the first cold rolling is completed, the second cold rolling is performed, and the steel strip passing through the large diameter work roll passes through the small diameter work roll with a roll diameter of 50 to 100 mm. The small diameter work roll with a roll diameter of 50 to 100 mm is an example of the second work roll involved in the present invention. In the second cold rolling, only the remaining strip thickness portion that was not completely rolled in the first cold rolling is rolled. The steel strip after the second cold rolling is a cold-rolled steel strip.

[0152] Here, the reason for performing the second cold rolling after the first cold rolling is explained. That is, when comparing the first cold rolling and the second cold rolling, if the rolling reduction of the two cold rollings is the same, the first cold rolling using the large-diameter work roll needs to have a larger rolling load than the second cold rolling using the small-diameter work roll. In addition, stainless steel is generally harder than ordinary steel, and the more the cold rolling enters the latter half of the treatment, the more work hardening will occur, and the strength of the steel strip will increase. According to these circumstances, if only the large-diameter work roll is used for cold rolling in the cold rolling step S4, the rolling load that must be applied to the steel strip will exceed the allowable range from the perspective of the manufacturability and productivity of the stainless steel until the desired strip thickness is obtained. Therefore, the first cold rolling is performed with the large-diameter work roll, and the second cold rolling is performed with the small-diameter work roll as in the present embodiment. In the present embodiment, among the small-diameter work rolls with a roll diameter of less than 200 mm, the work rolls with a roll diameter of 50 to 100 mm generally used as small-diameter work rolls are used as the second work rolls.

[0153] In addition, in the present embodiment, the second cold rolling is performed after the first cold rolling is performed in the cold rolling process S4, but the first cold rolling can also be performed after the second cold rolling. However, stainless steel is generally harder than ordinary steel. Furthermore, the more the cold rolling enters the latter half of the process, the more work hardening will occur, and the strength of the steel strip will increase. Therefore, if the first cold rolling is performed after the second cold rolling, in order to concentrate the rolling strain in the center of the plate thickness of the steel strip after the second cold rolling, it is necessary to have a rolling load greater than that of performing the second cold rolling after the first cold rolling. According to these circumstances, considering the manufacturability and productivity of this stainless steel, it is preferred to perform the second cold rolling after the first cold rolling as in the present embodiment.

[0154] <Annealing step S5>

[0155] Then, in the annealing step S5, the cold-rolled steel strip manufactured in the cold-rolling step S4 is annealed at a temperature higher than the recrystallization start temperature and lower than Ac1. The annealing performed in the annealing step S5 is a finishing annealing for the purpose of completing the recrystallization of the ferrite phase and eliminating the martensite phase in the cold-rolled steel strip. The finishing annealing performed in the annealing step S5 is composed of a heating process, a soaking process, and a cooling process, similar to the softening annealing in the softening annealing step S3.

[0156] During the heating process, the cold-rolled steel strip is heated to a temperature above the start temperature of recrystallization and below Ac1 at a heating rate of less than 50°C / s. By setting the heating rate to less than 50°C / s, the martensite phase can be eliminated during the heating process. During the soaking process, the cold-rolled steel strip after the heating process is soaked for more than 5 seconds at a temperature above the start temperature of recrystallization and below Ac1. In the present embodiment, the start temperature of recrystallization is set to 800°C. By setting the start time of recrystallization to 800°C, the recrystallization of the ferrite phase can be completed within a short soaking time. However, the start temperature of recrystallization is not limited to 800°C, and the start temperature of recrystallization can also be set to, for example, a temperature lower than 800°C. On the other hand, by setting the upper limit of the soaking temperature to a temperature below Ac1, the generation of a new martensite phase in the cold-rolled steel strip can be prevented, and the remaining martensite phase in the cold-rolled steel strip can be substantially eliminated.

[0157] In the cooling process, the cold-rolled steel strip after the soaking process is cooled at a cooling rate of 50°C / s or less. By cooling at a cooling rate of 50°C / s or less, the martensite phase can also be eliminated during the cooling process. By performing the final annealing consisting of the relevant treatments on the cold-rolled steel strip, the completion of the recrystallization of the ferrite phase in the cold-rolled steel strip and the elimination of the martensite phase can be effectively achieved in the annealing step S5. By completing the annealing step S5, the stainless steel as the final product is obtained, and the manufacture of the stainless steel is completed.

[0158] 〔Summarize〕

[0159] The ferritic stainless steel according to the present invention may further contain, in mass %, one or more selected from Mo: 0.50% or less, Cu: 1.0% or less, O: 0.01% or less, V: 0.15% or less, B: 0.10% or less, and Ti: 0.50% or less.

[0160] The ferritic stainless steel according to the aspect of the present invention may further contain, in terms of mass%, one or more selected from Co: 0.01% to 0.50%, Zr: 0.01% to 0.10%, Nb: 0.01% to 0.10%, Mg: 0.0005% to 0.003%, Ca: 0.0003% to 0.003%, Y: 0.01% to 0.20%, rare earth metals other than Y: a total of 0.01% to 0.10%, Sn: 0.001% to 0.50%, Sb: 0.001% to 0.50%, Pb: 0.01% to 0.10%, and W: 0.01% to 0.50%.

[0161] The steel billet in the method for producing ferritic stainless steel according to the technical solution of the present invention may further contain, in terms of mass %, one or more selected from the group consisting of Mo: 0.50% or less, Cu: 1.0% or less, O: 0.01% or less, V: 0.15% or less, B: 0.10% or less, and Ti: 0.50% or less.

[0162] The steel billet in the method for producing ferritic stainless steel according to the technical aspect of the present invention may further contain, in terms of mass%, one or more selected from Co: 0.01% to 0.50%, Zr: 0.01% to 0.10%, Nb: 0.01% to 0.10%, Mg: 0.0005% to 0.003%, Ca: 0.0003% to 0.003%, Y: 0.01% to 0.20%, rare earth metals other than Y: a total of 0.01% to 0.10%, Sn: 0.001% to 0.50%, Sb: 0.001% to 0.50%, Pb: 0.01% to 0.10%, and W: 0.01% to 0.50%.

[0163] [Appendix]

[0164] The present invention is not limited to the present embodiment, and various modifications can be made within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in each embodiment are also included in the technical scope of the present invention.

[0165] [Example]

[0166] The evaluation results of the ferritic stainless steel involved in the embodiments and comparative examples of the present invention are described below. Hereinafter, the ferritic stainless steel involved in the embodiments of the present invention is referred to as "invention steel", and the ferritic stainless steel involved in the comparative examples of the present invention is referred to as "comparative steel". In this embodiment, first, 5 types of steel billets having any one of the compositions A to E shown in Table 1 below are manufactured by smelting in an actual operating production line. The content of each element constituting the compositions A to E is within the numerical range of the content of each element contained in the ferritic stainless steel involved in the technical solution of the present invention. In addition, Table 1 also lists the values ​​of Ac1 in each case of the compositions A to E.

[0167]

Table 1

[0168]

[0169] As shown in Table 1, the index values ​​of the invention steel and the comparative steel produced based on the steel billet having the composition E were 85, which was a result exceeding the upper limit of the preferred numerical range of 50 in the present invention. Such a result was presumably because the content of Cr in the composition E, which affects the index value, was 12.5%.

[0170] Next, the steel slabs of each composition were hot rolled to produce hot-rolled steel strips of each composition with a plate thickness of 3 mm and a plate width of 150 mm. Subsequently, the hot-rolled steel strips of each composition were subjected to softening annealing and cold rolling under the "actual conditions" shown in Table 2 below to produce cold-rolled steel strips of each composition with a plate thickness of 1 mm and a plate width of 150 mm. Then, the cold-rolled steel strips of each composition were finished annealed to produce the first to seventh invention steels and the first to eighteenth comparative steels.

[0171]

Table 2

[0172]

[0173] Table 2 also shows the "recommended conditions" for softening annealing and cold rolling. The conditions described in the "recommended conditions" column of Table 2 are the same as the conditions of the present embodiment. In addition, the "lower limit temperature" in the "softening annealing" column of the "recommended conditions" indicates the lower limit value of the maximum annealing temperature, and the "upper limit temperature" in the same column indicates the upper limit value of the maximum annealing temperature. The values ​​described in the "lower limit temperature" and "upper limit temperature" columns are calculated by substituting the value (942) of Ac1 of composition A into the formula of 0.76×Ac1+201°C or more and 1050°C or less for each invention steel and each comparative steel of composition A. On the other hand, for each invention steel and each comparative steel of composition B to E, the values ​​(811, 855, 920, 710) of Ac1 of composition B to E are calculated by substituting the values ​​(811, 855, 920, 710) of Ac1 of composition B to E into the formula of 0.76×Ac1+201°C or more and 1.10×Ac1-56°C or less.

[0174] In addition, the above-mentioned Table 2 also shows the "characteristic evaluation" and "comprehensive evaluation" for each of the 1st to 7th invention steels and the 1st to 18th comparative steels. The "corrugation height" column of the "characteristic evaluation" shows the measurement result of the corrugation height of the wrinkles. In addition, the "r value" column of the "characteristic evaluation" shows the calculation result of the r value. In addition, the method for measuring the corrugation height of the wrinkles and the method for calculating the r value are the same methods as those in the present embodiment. In the "comprehensive evaluation", the case where the corrugation height of the wrinkles is less than 15μm, the r value is greater than 0.9, and the second martensite area ratio is greater than 0% and less than 1.0% is evaluated as "○". On the other hand, if any of the following conditions is met: the corrugation height of the wrinkles is greater than 15μm, the r value is less than 0.9, or the second martensite area ratio is greater than 1.0%, it is evaluated as "×".

[0175] The underlined values ​​in Table 2 indicate values ​​outside the preferred numerical range of the present embodiment. In addition, the underlined "×" in Table 2 indicates that the cold rolling rate after all passes is less than 50% of the total cold rolling rate.

[0176] As shown in Table 2, the corrugation height of the wrinkles of the 1st, 9th, 11th, 13th, and 16th comparative steels is higher than 15 μm, so the comprehensive evaluation is "×". The corrugation height of the wrinkles is higher than 15 μm, which is estimated to be because the first martensite area ratio is less than 5.0% in any of the 1st, 9th, 11th, 13th, and 16th comparative steels. In other words, it is estimated that the increase in the amount of crystal clusters in the steel exceeds the allowable range for improving the wrinkle resistance, resulting in the corrugation height of the wrinkles being higher than 15 μm.

[0177] In addition, as shown in Table 2, for each comparative steel other than the 1st, 9th and 18th comparative steels, the r value is less than 0.9, so the comprehensive evaluation becomes "×". The reason why the r value is less than 0.9 is speculated as follows. First, for the 2nd and 3rd comparative steels, the 5th to 8th comparative steels, the 10th to 13th comparative steels and the 16th comparative steel, it is speculated that they meet at least one of the total cold rolling rate less than 60%, the cold rolling rate of each pass less than 15%, and the cold rolling rate after all passes is less than 50% of the total cold rolling rate. In other words, for any of the 2nd and 3rd comparative steels, the 5th to 8th comparative steels, the 10th to 13th comparative steels and the 16th comparative steel, it is speculated that the concentration of rolling strain does not sufficiently occur in the center of the plate thickness of these comparative steels, so the r value becomes less than 0.9.

[0178] Next, for the 14th and 15th comparative steels, it is estimated that the first martensite area ratio is greater than 30.0%. That is, for both the 14th and 15th comparative steels, it is estimated that the martensite phase increases more than necessary, the ductility decreases, and therefore the r value becomes less than 0.9. Next, for the 17th comparative steel, it is estimated that in addition to the total cold rolling rate being less than 60%, the first martensite area ratio is also greater than 30.0%, and therefore the r value becomes less than 0.9.

[0179] Furthermore, as shown in Table 2, the 14th, 15th, 17th, and 18th comparative steels had a second martensite area ratio of 1.0% or more, and thus were rated "×" in the comprehensive evaluation.

[0180] On the other hand, regarding the 1st to 7th invention steels, the characteristics of the 3rd and 4th invention steels are evaluated as the best results among all invention steels. Specifically, the corrugation height of the wrinkles of the 3rd invention steel ranks third lowest among all invention steels (2.39μm). The reason for this result is speculated to be that the first martensite area ratio ranks third highest among all invention steels (9.44%). In addition, the r value of the 3rd invention steel is the largest among all invention steels (1.12). The reason for this result is speculated to be that the total cold rolling rate is the highest among all invention steels (85%). Furthermore, the second martensite area ratio of the 3rd invention steel ranks fourth lowest among all invention steels (0.17%).

[0181] The corrugation height of the wrinkles of the fourth invention steel is the lowest among all invention steels (2.28μm). In addition, the r value of the fourth invention steel is the fourth largest among all invention steels (0.93). This result is presumably because the total cold rolling rate is the fourth highest among all invention steels (69%). Furthermore, the second martensite area ratio of the fourth invention steel is the third lowest among all invention steels (0.15%).

[0182] Possibility of Industrial Application

[0183] The present invention can be used for ferritic stainless steel and a method for producing ferritic stainless steel.

[0184] Explanation of symbols

[0185] S1 Melting Process

[0186] S2 Hot rolling process

[0187] S3 Softening Annealing Process

[0188] S4 Cold rolling process

[0189] S5 Annealing process

Claims

1. Ferritic stainless steel containing, by mass%, C: 0.063% to 0.12%, Si: 1.0% to 1.0%, Mn: 1.0% to 1.0%, Ni: 1.0% to 1.0%, Cr: 12.0% to 18.0%, N: 0.10% to 0.50% to 0.50%, the remainder being Fe and unavoidable impurities, When measuring the surface properties of wrinkles formed by a tensile test in which a tensile strain of 16% is applied to the ferritic stainless steel in a tensile direction parallel to the rolling direction, the corrugation height of the wrinkles represented by the average height of the waviness curve elements is 7.54 μm or less, and the r value is greater than 0.9, and the steel contains a martensite phase whose area ratio in a cross section cut along a plane parallel to the rolling direction and perpendicular to the width direction is greater than 0% and less than 1.0%.

2. The ferritic stainless steel according to claim 1, wherein: The metal further contains, in terms of mass%, one or more selected from the group consisting of Mo: 0.50% or less, Cu: 1.0% or less, O: 0.01% or less, V: 0.15% or less, B: 0.10% or less, and Ti: 0.50% or less.

3. The ferritic stainless steel according to claim 1 or 2, wherein: The alloy further contains, in terms of mass%, one or more selected from Co: 0.01% to 0.50%, Zr: 0.01% to 0.10%, Nb: 0.01% to 0.10%, Mg: 0.0005% to 0.003%, Ca: 0.0003% to 0.003%, Y: 0.01% to 0.20%, rare earth metals other than Y: a total of 0.01% to 0.10%, Sn: 0.001% to 0.50%, Sb: 0.001% to 0.50%, Pb: 0.01% to 0.10%, and W: 0.01% to 0.50%.

4. A method for producing ferritic stainless steel, wherein the ferritic stainless steel is subjected to a tensile test in which a tensile strain of 16% is applied to the ferritic stainless steel in a tensile direction parallel to a rolling direction, and the corrugation height of the corrugation represented by the average height of the corrugation curve element when measuring the surface properties of the corrugation is 15 μm or less, and the r value is 0.9 or more, and the steel contains a martensite phase whose area ratio in a cross section cut along a plane parallel to the rolling direction and perpendicular to the width direction is greater than 0% and less than 1.0%; the method comprising: A hot rolling step of hot rolling a steel billet containing, by mass%, C: 0.12% or less, Si: 1.0% or less, Mn: 1.0% or less, Ni: 1.0% or less, Cr: 12.0% or more and 18.0% or less, N: 0.10% or less, and Al: 0.50% or less, with the remainder being Fe and unavoidable impurities, to produce a hot-rolled steel strip; a softening annealing step of annealing the hot-rolled steel strip produced in the hot rolling step to soften it, thereby producing the hot-rolled annealed steel strip having an area ratio of 5.0% or more and 30.0% or less of a martensite phase in a cross section cut along a plane parallel to the rolling direction and perpendicular to the width direction of the hot-rolled annealed steel strip, and a remainder other than the martensite phase including a ferrite phase; and a cold rolling step of cold rolling the hot-rolled annealed steel strip produced in the softening annealing step to produce a cold-rolled steel strip; In the cold rolling process, The total cold rolling ratio, which is the ratio of the difference between the thickness of the hot-rolled annealed steel strip and the thickness of the cold-rolled steel strip to the thickness of the hot-rolled annealed steel strip, is set to 60% or more. For the hot rolled annealed steel strip, (i) using a first working roll having a roll diameter of 200 mm or more, cold rolling is performed in such a manner that the cold rolling rate per pass is 15% or more and the cold rolling rate after all passes is 50% or more of the total cold rolling rate, and then, (ii) Cold rolling is further performed using a second work roll having a roll diameter of less than 200 mm.

5. The method for producing ferritic stainless steel according to claim 4, wherein: The steel slab further contains, in terms of mass%, one or more selected from the group consisting of Mo: 0.50% or less, Cu: 1.0% or less, O: 0.01% or less, V: 0.15% or less, B: 0.10% or less, and Ti: 0.50% or less.

6. The method for producing ferritic stainless steel according to claim 4 or 5, wherein: The steel slab further contains, in terms of mass%, one or more selected from Co: 0.01% to 0.50%, Zr: 0.01% to 0.10%, Nb: 0.01% to 0.10%, Mg: 0.0005% to 0.003%, Ca: 0.0003% to 0.003%, Y: 0.01% to 0.20%, rare earth metals other than Y: a total of 0.01% to 0.10%, Sn: 0.001% to 0.50%, Sb: 0.001% to 0.50%, Pb: 0.01% to 0.10%, and W: 0.01% to 0.50%.

Citation Information

Patent Citations

  • Production of thin ferritic stainless steel sheet having excellent processability

    JP1984107030A

  • Ferritic stainless steel sheet excellent in formability and ridging resistance, and its production

    JP1998130786A

  • Ferrite stainless steel cold-rolled steel band and manufacturing method thereof

    CN101649418A

  • Ferritic stainless steel sheet and method for manufacturing same

    CN107709592A

  • Ferrite stainless steel with excellent ridging property and surface quality and manufacturing method therefor

    CN110073022A