A biorepair membrane loaded with vascular endothelial growth factor and preparation method thereof
The vascular endothelial growth factor and animal-derived biofilm materials are fully mixed through the electrospinning method to prepare a porous three-dimensional biorepair membrane, which solves the problem of poor factor loading of traditional cardiovascular patch materials and realizes the factor loading during the entire repair process. The sustained release and cardiovascular and cerebrovascular repair effects are improved.
Patent Information
- Application Number
- CN202310028828.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-09
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-01-09
AI Technical Summary
Traditional cardiovascular patch materials cannot effectively load vascular endothelial growth factors, so the factors can only play a role in the initial cardiovascular and cerebrovascular repair, and the loading effect is poor and cannot continue to play a repair role.
The animal-derived biofilm material and vascular endothelial growth factor solution were thoroughly mixed using the electrospinning method to prepare a porous three-dimensional biorepair membrane to improve the binding effect of the factors and tissue scaffolds.
It achieves sustained and effective release of vascular endothelial growth factors throughout the entire repair process, improves cardiovascular and cerebrovascular repair effects, and reduces immune rejection.
Smart Images

Figure CN115920136B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of biorepair materials, and in particular to a biorepair membrane loaded with vascular endothelial growth factor and a preparation method thereof. Background Art
[0002] Cardiovascular patches are commonly used patch materials in surgical repair of cardiovascular and cerebrovascular diseases, including heart patches and vascular patches. Heart patches are used to repair ventricular diseases such as ventricular septal defects and ventricular wall repairs. They are also commonly used in repair surgeries for atrial diseases such as atrial septal defects; vascular patches are used to repair vascular fistulas caused by hemangiomas, vascular stenosis, and other reasons. Commonly used materials for traditional cardiovascular patches include autologous tissue, artificial synthetic materials (commonly polyester materials, polytetrafluoroethylene materials), and animal-derived biomembrane materials (such as bovine pericardium materials); among them, autologous tissue is greatly restricted in terms of material sources, while artificial synthetic materials and animal-derived biomembrane materials lack tissue reconstruction capabilities and cannot meet different application requirements.
[0003] With the rise and development of tissue engineering technology, degradable biomaterials are gradually being used to replace traditional patch materials. The degradable biomaterial can provide complete structural support for cell growth and plays a very critical role in the construction of new tissues, so it is also called a degradable "scaffold". At present, biomaterials related to cardiovascular tissue engineering products include gelatin, chitosan, collagen, fibrin, decellularized tissue (such as small intestinal submucosa, etc.), decellularized membranes (fish scales, pig skin, bovine pericardium, and animal tissues, etc.), etc.; in order to further improve the repair effect and effect of biological tissue on cardiovascular, the corresponding biomaterials and growth factors can be further loaded on the tissue scaffold. For example, Chinese patent document CN201710756877.7 discloses an intelligent tissue engineering patch, which uses bovine pericardium as a raw material to prepare a tissue engineering patch, and then the patch is immersed in a vascular endothelial growth factor (VEGF) sustained-release microsphere solution, and finally freeze-dried, and the decellularized bovine pericardium scaffold and sustained-release microspheres are combined to produce an intelligent tissue engineering patch with sustained-release function. Another Chinese patent document CN201510245387.1 discloses a biorepair membrane and a preparation method thereof, wherein an animal-derived membrane tissue is decellularized and deantigenized to obtain a decellularized matrix, which is then coated with a natural polymer material coating and finally placed in a freeze dryer for freeze drying to complete the preparation of the biorepair membrane.
[0004] However, whether it is freeze-dried after soaking or freeze-dried after coating, there is a problem that the growth factor cannot effectively enter the interior of the tissue scaffold, and is only loaded and bound on the shallow surface of the tissue scaffold, resulting in the growth factor only being effective in the early stage of cardiovascular and cerebrovascular repair, and not being able to continue to play an effective role in the entire repair process as the biorepair membrane degrades. At the same time, there are also problems such as poor binding between the loading factor material and the tissue scaffold and low effective loading amount. Summary of the invention
[0005] In view of the above problems, the present invention provides a biorepair membrane loaded with vascular endothelial growth factor and a preparation method thereof, wherein the biorepair membrane is prepared by electrospinning after the biorepair membrane is fully mixed with a vascular endothelial growth factor (VEGF) solution, thereby improving the binding effect between the loaded factor and the tissue scaffold. The specific technical scheme is as follows:
[0006] Firstly, the present invention provides a biorepair membrane loaded with vascular endothelial growth factor, which is prepared by an electrostatic spinning method by freeze-drying and crushing an animal-derived biomembrane material and dissolving the vascular endothelial growth factor in a polypyrrole solution as a spinning solution.
[0007] The aforementioned biological repair loaded with vascular endothelial growth factor, the animal-derived biomembrane material includes but is not limited to bovine or porcine pericardium, small intestinal submucosa and bladder material.
[0008] Secondly, the present invention provides a method for preparing a vascular endothelial growth factor-loaded biorepair membrane, comprising the following steps:
[0009] 1) Raw material pretreatment: Clean the animal-derived biofilm material to remove surface dirt;
[0010] 2) Degreasing: Soak the pretreated animal-derived biofilm material in a degreasing agent, shake and degrease, and use purified water to clean the reagent residue;
[0011] 3) Virus removal: Soak the defatted animal-derived biofilm material in NaOH or hydrogen peroxide, continue to shake to remove the virus, and then use purified water to clean the reagent residue;
[0012] 4) Freeze-drying: Spread the virus-free animal-derived biofilm material flat in a container and freeze-dry it using a freeze dryer;
[0013] 5) Crushing: crush the freeze-dried animal-derived biofilm material using a crusher for later use;
[0014] 6) Preparing a spinning solution: dissolving VEGF and crushed animal-derived biofilm materials in a polypyrrole solution by an ultrasound-assisted method to prepare a spinning solution;
[0015] 7) Electrospinning: Control the spinning voltage, injection speed and the distance between the roller and the needle to perform electrospinning into a porous three-dimensional scaffold to obtain a biorepair membrane loaded with vascular endothelial growth factor.
[0016] In the aforementioned method for preparing a bioremediation membrane loaded with vascular endothelial growth factor, in step 2), the degreasing reagent is selected from one or more of n-hexane, sodium dodecyl sulfate with a mass fraction concentration of 0.4%, a mixture of chloroform and methanol, and isopropanol; the degreasing treatment method is as follows: the animal-derived biomembrane material is mixed in a ratio of weight to volume of the degreasing reagent = 1:10-20, and the mixture is shaken at a speed of 100 rpm for 48-56 hours, and then the reagent residue is cleaned with purified water.
[0017] In the aforementioned method for preparing a vascular endothelial growth factor-loaded biorepair membrane, in step 3), the concentration of NaOH used for virus removal is 0.25-1.5 mol / L; the mass fraction concentration of hydrogen peroxide used is 5%-8%.
[0018] In the aforementioned method for preparing a vascular endothelial growth factor-loaded bioremediation membrane, in step 3), the deviral treatment method is as follows: the animal-derived biomembrane material is mixed at a weight ratio of 1:10 to 20 to the reagent volume, and the mixture is shaken at 100 rpm for 48 to 56 hours, and then the reagent residue is washed with purified water; the freeze-drying conditions are set as follows: pre-freezing at -20°C for 12 to 18 hours, and then freeze-drying at -60°C for 48 to 72 hours.
[0019] In the aforementioned method for preparing the vascular endothelial growth factor-loaded biorepair membrane, in step 5), the particle size of the animal-derived biomembrane material is crushed to less than 500 μm.
[0020] In the aforementioned method for preparing a vascular endothelial growth factor-loaded biorepair membrane, in step 6), in the spinning solution, the volume ratio of the crushed animal-derived biomembrane material to the polypyrrole solution is 1:20 to 1:10, and the amount of VEGF added is 10,000 to 50,000 IU per 100 ml of the mixture of animal-derived biomembrane material and polypyrrole solution.
[0021] In the aforementioned method for preparing a vascular endothelial growth factor-loaded biorepair membrane, in step 7), the electrospinning voltage is 15 to 25 kV, the injection speed V is 0.02 to 0.04 mm / min, and the distance between the roller and the needle is 20 to 30 cm.
[0022] The porous three-dimensional scaffold structure of the aforementioned vascular endothelial growth factor-loaded biorepair membrane is specifically formed by stacking multiple electrospun layers, each electrospun layer is formed by a spinning strand in an S-shaped equal inter-disk fold, and the spinning strands between the electrospun layers are stacked in a positive direction.
[0023] The beneficial effects of the present invention are:
[0024] 1) The present invention effectively combines the biofilm with vascular endothelial growth factor (VEGF) to achieve the healing, repair and regeneration of damaged cardiovascular and cerebrovascular tissues, thereby improving the cardiovascular and cerebrovascular repair effect.
[0025] 2) The present invention prepares a biorepair membrane by using an electrospinning method after fully mixing the biofilm with a vascular endothelial growth factor (VEGF) solution, thereby improving the binding effect between the loading factor and the tissue scaffold, rather than just staying at the binding with the surface of the tissue scaffold, so that VEGF continues to play an effective role in the entire repair process as the biorepair membrane degrades.
[0026] 3) The present invention prepares a porous three-dimensional scaffold by an electrospinning method, and the internal pores are interconnected to form an open pore structure, which provides sufficient adhesion space for cells and facilitates the transmission of nutrients and metabolites.
[0027] 4) The present invention uses decellularization technology to remove the immunogenicity of animal-derived biofilm materials, thereby reducing the immune rejection reaction after implantation in the body. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The schematic diagram is a structural diagram of the vascular endothelial growth factor-loaded biorepair membrane of the present invention. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the present invention more clear, the technical solution of the present invention will be clearly and completely described below in conjunction with embodiments and drawings.
[0030] Example 1
[0031] This example is to prepare a biorepair membrane loaded with vascular endothelial growth factor, such as Figure 1 As shown, the biorepair membrane is prepared by electrospinning after freeze-dried and crushed bovine pericardium and vascular endothelial growth factor is dissolved in a polypyrrole solution as a spinning solution. The preparation method includes the following steps:
[0032] 1) Raw material pretreatment: Preliminary cleaning of bovine pericardium to remove surface dirt.
[0033] 2) Degreasing: A mixture of chloroform and methanol (the volume ratio of chloroform to methanol is 2:1) is used as the degreasing reagent. The pretreated bovine pericardium is immersed in the degreasing reagent at a volume ratio of bovine pericardium to the reagent = 1:10, and shaken at 100 rpm for 48 hours, and then the reagent residue is washed with purified water.
[0034] 3) Virus removal: Soak the defatted bovine pericardium in 1 mol / L NaOH, with the weight of bovine pericardium to the volume of NaOH = 1:20, then shake it at 100 rpm for 50 h, and then use purified water to clean the reagent residue.
[0035] 4) Freeze-drying: Spread the devirioned bovine pericardium flat in a container, pre-freeze it at -20°C for 12 hours using a freeze dryer, and then freeze-dry it at -60°C for 48 hours;
[0036] 5) Grinding: The freeze-dried bovine pericardium is pulverized using a pulverizer to a particle size of 400 μm.
[0037] 6) Preparation of spinning solution: VEGF and crushed bovine pericardium were dissolved in a polypyrrole solution by ultrasound-assisted method to prepare spinning solution; the volume ratio of bovine pericardium to polypyrrole solution was 1:10, and the amount of VEGF was 35000 IU per 100 ml of solution.
[0038] 7) Electrospinning: The control voltage was 18 kV, the injection speed V was 0.02 mm / min, and the distance between the roller and the needle was 20 cm. A porous three-dimensional scaffold was made, such as Figure 1 As shown, it is a biorepair membrane loaded with vascular endothelial growth factor. The biorepair membrane loaded with vascular endothelial growth factor is specifically formed by stacking multiple electrospun layers, each electrospun layer is spun in an S-shaped equilateral disc formation, and the spinning of the electrospun layers is stacked in a positive direction to form a porous three-dimensional scaffold, which is interconnected to form an open pore structure, providing sufficient adhesion space for cells and facilitating the transmission of nutrients and metabolites.
[0039] Example 2
[0040] This embodiment also prepares a biorepair membrane loaded with vascular endothelial growth factor, which is prepared by electrospinning the pig small intestinal submucosal layer after freeze-drying and crushing and dissolving the vascular endothelial growth factor in a polypyrrole solution as a spinning solution. The preparation method includes the following steps:
[0041] 1) Raw material pretreatment: Preliminary cleaning of the submucosa of the pig small intestine to remove surface dirt.
[0042] 2) Degreasing: Sodium dodecyl sulfate with a mass fraction concentration of 0.4% was selected as the degreasing agent. The pretreated pig small intestinal submucosal layer was immersed in the degreasing agent at a volume ratio of 1:20, and the degreasing agent was shaken at 100 rpm for 52 hours, and then the reagent residue was washed with purified water.
[0043] 3) Virus removal: Soak the defatted porcine small intestinal submucosa in 1.5 mol / L NaOH, with the weight of the porcine small intestinal submucosa to the volume ratio of NaOH = 1:15, then shake it at 100 rpm for 55 h, and then use purified water to clean the reagent residue.
[0044] 4) Freeze-drying: Spread the virus-free porcine small intestinal submucosal layer flat in a container, pre-freeze at -20°C for 15 hours using a freeze dryer, and then freeze-dry at -60°C for 60 hours;
[0045] 5) Grinding: The freeze-dried porcine small intestinal submucosa is pulverized using a pulverizer to a particle size of 300 μm.
[0046] 6) Preparation of spinning solution: VEGF and crushed porcine small intestinal submucosa were dissolved in polypyrrole solution by ultrasound-assisted method to prepare spinning solution; the volume ratio of porcine small intestinal submucosa to polypyrrole solution was 1:15, and 47,000 IU of VEGF was added per 100 ml of solution.
[0047] 7) Electrospinning: The control voltage was 20 kV, the injection speed V was 0.03 mm / min, and the distance between the roller and the needle was 25 cm. A porous three-dimensional scaffold was made, which was the vascular endothelial growth factor-loaded biorepair membrane.
[0048] Example 3
[0049] This embodiment also prepares a biorepair membrane loaded with vascular endothelial growth factor, which is prepared by electrospinning a pig bladder material that is freeze-dried and crushed and dissolved with vascular endothelial growth factor in a polypyrrole solution as a spinning solution. The preparation method includes the following steps:
[0050] 1) Raw material pretreatment: The pig bladder material is preliminarily cleaned to remove surface dirt.
[0051] 2) Degreasing: n-hexane was used as the degreasing agent. The pretreated pig bladder material was immersed in the degreasing agent at a volume ratio of 1:15, and the material was shaken at 100 rpm for 56 hours, and then the reagent residue was washed with purified water.
[0052] 3) Virus removal: Soak the defatted porcine bladder material in 6% hydrogen peroxide (weight to volume ratio = 1:20), then shake at 100 rpm for 56 h, and then use purified water to clean the reagent residue.
[0053] 4) Freeze-drying: Spread the virus-free pig bladder material flat in a container, pre-freeze it at -20°C for 18 hours using a freeze dryer, and then freeze-dry it at -60°C for 72 hours;
[0054] 5) Grinding: The freeze-dried pig bladder material is pulverized using a grinder to a particle size of 350 μm.
[0055] 6) Preparation of spinning solution: VEGF and crushed porcine bladder material were dissolved in polypyrrole solution by ultrasound-assisted method to prepare spinning solution; the volume ratio of porcine bladder material to polypyrrole solution was 1:20, and 12000 IU of VEGF was added per 100 ml of solution.
[0056] 7) Electrospinning: The control voltage was 25 kV, the injection speed V was 0.04 mm / min, and the distance between the roller and the needle was 30 cm. A porous three-dimensional scaffold was made, which was the vascular endothelial growth factor-loaded biorepair membrane.
[0057] Example 4 Effect Example
[0058] This example uses the vascular endothelial growth factor-loaded biorepair membrane prepared in Example 1 to perform cardiovascular patch surgery on mice.
[0059] At the same time, the following two engineering patches are used as comparison examples:
[0060] Comparative Example 1: After preliminary cleaning, degreasing, and virus removal, the bovine pericardium was soaked in a vascular endothelial growth factor (VEGF) solution for 48 hours, and finally freeze-dried to obtain a comparative vascular patch 1. During the preparation of comparative vascular patch 1, the cleaning, degreasing, and virus removal treatments were consistent with those of Example 1. The concentration of the vascular endothelial growth factor (VEGF) solution used for soaking was 35,000 IU of VEGF per 100 ml, and the volume ratio of bovine pericardium to VEGF solution was 1:10. A freeze dryer was used to pre-freeze at -20°C for 18 hours, and then freeze-dried at -60°C for 72 hours.
[0061] Comparative Example 2: The bovine pericardium was preliminarily cleaned, decellularized and deantigenized to obtain a decellularized matrix, and then coated with vascular endothelial growth factor (VEGF) on the outside, and finally placed in a freeze dryer for freeze drying to obtain a comparative vascular patch 2. During the preparation of comparative vascular patch 2, the cleaning, degreasing and virus removal treatments were consistent with those of Example 1. The concentration of the coated vascular endothelial growth factor (VEGF) solution was 35000 IU of VEGF per 100 ml, and the coating thickness was 0.5 mm. The freeze dryer was used to pre-freeze at -20°C for 18 hours, and then freeze-dried at -60°C for 72 hours.
[0062] The specific process of cardiovascular patch surgery in mice is as follows:
[0063] Before the patch transplantation, the nude rats were fasted for 12 hours and had free access to water. After the nude rats were weighed, anesthesia was injected into the abdominal cavity. An incision was made longitudinally in the lower abdomen along the midline of the abdomen, and the subcutaneous tissue and muscle were cut along the midline to enter the abdominal cavity. The intestinal tract was carefully removed from the body, and the retroperitoneum was carefully separated with hemostatic forceps to expose the abdominal aorta and its branches. A section of the abdominal aorta from below the renal artery to the bifurcation of the iliac vessels was freed, and the proximal and distal ends were clamped with artery clamps. Part of the aortic wall was cut off in the middle of the abdominal aorta to establish an abdominal aorta defect model. The vascular patch was trimmed to a suitable size under a surgical magnifying glass. The experimental group used the vascular endothelial growth factor-loaded biorepair membrane prepared in Example 1, and the control group used the vascular patches prepared in Comparative Example 1 and Comparative Example 2, respectively. The aortic patch was anastomosed with the defective abdominal aorta by continuous suture. After the anastomosis, the distal artery clamp was opened first, the posterior peritoneum was closed, the intestine was brought into the abdominal cavity and repositioned, and levofloxacin hydrochloride was added to the drinking water of the nude rats after transplantation to prevent postoperative infection. 28 days after surgery, the nude rats were anesthetized by intraperitoneal injection, the abdomen was cut open, the adhesion tissue was carefully separated, the abdominal aorta and the patch transplantation site were found, the two ends were blocked with artery clamps, the blood vessels with the patch were quickly cut off, and pathological examinations were performed respectively. The results are shown in Table 1.
[0064] Table 1. Repair status of cardiovascular patch surgery in mice
[0065]
[0066] The inspection results in Table 1 show that the inner surface of the two engineering patches of Comparative Examples 1 and 2 is rough. The microscopic structure of the blood vessels of Comparative Blood Vessel Patch 1 is loosely arranged and broken after surgery. The inner membrane of the microscopic structure of the blood vessels of Comparative Blood Vessel Patch 2 is incomplete, there is no continuous cell structure, and small thrombi are formed. After the cardiovascular patch surgery, the biorepair membrane loaded with vascular endothelial growth factor prepared by the present invention is smooth on the inner surface of the patch, no thrombus will be generated, and the endothelial cells are arranged neatly and continuously, which is equivalent to the structure of the autologous aorta. The reason is speculated to be: first, compared with the two comparative examples, the effective amount of VEGF in the biorepair membrane of the present invention is reorganized, and the loading factor is deeply combined with the stent, which can continue to play an effective role in the process of vascular repair; secondly, the porous three-dimensional stent of the biorepair membrane of the present invention is interconnected to form an open pore structure, which provides sufficient adhesion space for cells, and is conducive to the transmission of nutrients and metabolites, and is conducive to vascular repair.
[0067] It is obvious to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be regarded as exemplary and non-restrictive from any point of view. In addition, it should be understood that although this specification is described in accordance with the implementation mode, it does not include only one technical solution. This narrative mode of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole, and the technical solutions in the embodiments can also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for preparing a biorepair membrane loaded with vascular endothelial growth factor, characterized in that: The biorepair membrane is prepared by an electrostatic spinning method after freeze-drying and crushing animal-derived biomembrane materials and dissolving them in a polypyrrole solution with vascular endothelial growth factor (VEGF) as a spinning solution; the animal-derived biomembrane material includes bovine or porcine pericardium, small intestinal submucosa or bladder material; the biorepair membrane loaded with vascular endothelial growth factor is a porous three-dimensional scaffold structure, which is formed by stacking multiple electrospinning layers, each electrospinning layer is formed by a spinning in an S-shaped equal interspinning fold, and the spinning between the electrospinning layers is positively intersected and superimposed; the preparation method of the biorepair membrane specifically includes the following steps: 1) Raw material pretreatment: Clean the animal-derived biofilm material to remove surface dirt; 2) Degreasing: Soak the pretreated animal-derived biofilm material in a degreasing agent, shake and degrease, and use purified water to clean the reagent residue; 3) Virus removal: Soak the defatted animal-derived biofilm material in NaOH or hydrogen peroxide, continue to shake to remove the virus, and then use purified water to clean the reagent residue; 4) Freeze-drying: Spread the virus-free animal-derived biofilm material flat in a container and freeze-dry it using a freeze dryer; 5) Crushing: crush the freeze-dried animal-derived biofilm material using a crusher for later use; 6) Preparing a spinning solution: dissolving VEGF and crushed animal-derived biomembrane material in a polypyrrole solution by an ultrasonic-assisted method to prepare a spinning solution; in the spinning solution, the volume ratio of the crushed animal-derived biomembrane material to the polypyrrole solution is 1:20 to 1:10, and the amount of VEGF is added in an amount of 10,000 to 50,000 IU per 100 ml of the mixture of the animal-derived biomembrane material and the polypyrrole solution; 7) Electrospinning: Control the spinning voltage, injection speed and the distance between the roller and the needle to perform electrospinning to form a porous three-dimensional scaffold and obtain a biorepair membrane loaded with vascular endothelial growth factor; the electrospinning voltage is 15 to 25 kV, the injection speed V is 0.02 to 0.04 mm / min, and the distance between the roller and the needle is 20 to 30 cm.
2. The method for preparing the vascular endothelial growth factor-loaded biorepair membrane according to claim 1, characterized in that: In step 2), the degreasing agent is selected from one or more of n-hexane, sodium dodecyl sulfate with a mass fraction concentration of 0.4%, a mixture of chloroform and methanol, and isopropanol; the degreasing treatment method is: mixing the animal-derived biofilm material in a weight ratio of 1:10 to 20, shaking at a speed of 100 rpm for 48 to 56 hours, and then using purified water to clean the reagent residue.
3. The method for preparing the vascular endothelial growth factor-loaded biorepair membrane according to claim 1, characterized in that: In step 3), the concentration of NaOH used for deviral treatment is 0.25-1.5 mol / L; the mass fraction concentration of hydrogen peroxide used is 5%-8%; the deviral treatment method is: mixing the animal-derived biofilm material in a weight ratio of 1:10-20 to the reagent volume ratio, shaking at 100 rpm for 48-56 hours, and then using purified water to clean the reagent residue.
4. The method for preparing the vascular endothelial growth factor-loaded biorepair membrane according to claim 1, characterized in that: In step 4), the freeze-drying conditions are set as: pre-freezing at -20°C for 12 to 18 hours, and then freeze-drying at -60°C for 48 to 72 hours.
5. The method for preparing the vascular endothelial growth factor-loaded biorepair membrane according to claim 1, characterized in that: In step 5), the animal-derived biofilm material is crushed to a particle size of <500 μm.
Citation Information
Patent Citations
Biological repair membrane and preparation method thereof
CN106310373A
Heterogenous intelligent tissue engineering patch
CN109420202A
Regenerated silk fibroin tissue engineering scaffold containing vascular endothelial growth factor and preparation method thereof
CN102488929A
Three dimensional porous polyurethane scaffold for repairing of central nerve injury and preparation method thereof
CN106890359A
Degradable drug-loaded controlled-release myocardial repair patch with multilevel structure