A catalyst for synthesizing a sustained-release reagent for novel coronavirus detection and its preparation method and application

By loading precious metals or non-precious metal catalysts on MXene/C3N4 support, the problems of high production cost of trimethylolamide and unstable product quality in the prior art are solved, and efficient and safe continuous preparation is achieved, which is suitable for industrial scale Production.

CN115920946BActive Publication Date: 2024-11-01XIAN CATALYST NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310103276.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-13
Publication Date
2024-11-01
Estimated Expiration
2043-02-13

AI Technical Summary

Technical Problem

In the prior art, trimethylolamide aminomethane has high production costs, unstable product quality, and the Rainey nickel catalyst used is flammable and is not suitable for industrial scale production.

Method used

The catalyst is prepared by a support MXene/C3N4-supported noble metal or non-precious metal catalyst by equal volume impregnation method and hydrothermal treatment. It is used to continuously prepare trimethylolamide in a fixed bed reactor, and the reaction conditions are controlled to achieve efficient production.

Benefits of technology

It has achieved efficient continuous preparation of trimethylolamide, with high catalytic activity, good selectivity, long stability, mild reaction conditions, high safety, low operating costs, and suitable for industrial scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115920946B_ABST
    Figure CN115920946B_ABST
Patent Text Reader

Abstract

This invention discloses a catalyst for synthesizing a sustained-release reagent used in the COVID-19 test, wherein the sustained-release reagent is tris(hydroxymethyl)aminomethane. The catalyst comprises a support and an active metal supported on the support. The active metal is a noble metal M1 or a non-noble metal M2. The support is MXene / C3N4. The noble metal M1 is Pd, Pt, Rh, or Ru, and the non-noble metal M2 is Cu, Fe, Ni, Mn, Co, Mg, La, or Sn. The loading of the noble metal M1 is 0.2%–1% by weight, the loading of the non-noble metal M2 is 0.2%–10%, and the remainder is the support. This invention also discloses a method for preparing the catalyst and its applications. The catalyst of this invention exhibits very high catalytic activity and stability, enabling the continuous production of tris(hydroxymethyl)aminomethane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of nitro reduction process in catalytic hydrogenation, and specifically relates to a catalyst for synthesizing trishydroxymethylaminomethane, a sustained-release reagent used for novel coronavirus detection, as well as a preparation method and application thereof. Background Art

[0002] Tris (Hydroxymethyl) Aminomethane (Tris for short), also known as tromethamine, is an organic compound with the molecular formula (HOCH2)3CNH2. It is an important organic chemical raw material widely used in leather chemical additives, surfactants, promoters, emulsifiers, acid gas absorbents, etc., and has been widely used internationally.

[0003] In addition, it is also the most common buffer component and titration standard in biochemistry and molecular biology experiments. It can effectively treat acidosis in patients with acute lung injury and induce the phospholipid bilayer membrane to form a single-layer membrane with a corrugated structure. As the new crown epidemic is raging around the world, nucleic acid testing has become a direct and effective means of epidemic prevention and control, and tris(hydroxymethylaminomethane) will be in great demand as a sustained-release reagent for nucleic acid testing. At present, my country does not have mature technology and large-scale production, so the market prospects of tris(hydroxymethylaminomethane) are very broad.

[0004] Patent CN 113200877 A uses a Raney nickel catalyst to produce tris(hydroxymethyl)aminomethane through an autoclave process, with a maximum molar yield of only 87%. The process uses an autoclave reactor and is operated intermittently, which is the main production process at present. This production method has the problems of high production cost, large labor demand, unstable product quality, and the Raney nickel catalyst used is flammable and not suitable for large-scale use, so it lacks industrial scale. Summary of the invention

[0005] In view of the defects of the prior art, the present invention provides a catalyst for continuously preparing tris(hydroxymethyl)aminomethane, and a preparation method and application thereof. The catalyst preparation process is green and safe, the process is controllable, and it has the characteristics of high activity, high selectivity and long stability, and can realize efficient and continuous large-scale preparation of tris(hydroxymethyl)aminomethane.

[0006] A catalyst for synthesizing a sustained-release reagent for detecting the new coronavirus, wherein the sustained-release reagent for detecting the new coronavirus is trishydroxymethylaminomethane, and the catalyst consists of a carrier and an active metal loaded on the carrier, wherein the active metal is a noble metal M1 or a non-noble metal M2, and the carrier is MXene / C3N4, the noble metal M1 is Pd, Pt, Rh or Ru, and the non-noble metal M2 is Cu, Fe, Ni, Mn, Co, Mg, La or Sn; based on the weight ratio of the catalyst, the loading amount of the noble metal M1 is 0.2%-1%, the loading amount of the non-noble metal M2 is 0.2%-10%, and the balance is the carrier.

[0007] Preferably, the loading amount of the precious metal M1 is 0.3%-0.7%, and the loading amount of the non-precious metal M2 is 0.5%-5%.

[0008] The method for preparing the catalyst for synthesizing the sustained-release reagent used for novel coronavirus detection comprises the following steps:

[0009] (1) Preparation of MXene: Take the MXene precursor MAX and add it to a mixed solution of concentrated hydrochloric acid and lithium fluoride, stir for 36-72 hours, centrifuge and wash, add liquid nitrogen to the precipitate, freeze it quickly, and then place it in a vacuum freeze dryer until constant weight is obtained to obtain foamy MXene;

[0010] (2) Preparation of carrier MXene / C3N4: dissolve dicyandiamide in ethanol, add the MXene thereto, disperse by ultrasonication, stir for 12-36 hours, keep at 150-225°C for 12-48 hours, take out and filter, dry the filter cake to constant weight, and then calcine to obtain a carrier MXene / C3N4 with a C3N4-coated MXene foam network structure;

[0011] (3) Preparation of catalyst: Prepare an aqueous solution of active metal M by equal volume impregnation method, adjust the pH to 1.8-3.6, add the carrier MXene / C3N4 thereto, stir evenly, impregnate for 12-36 hours, dry to constant weight, calcine, and then reduce in a tubular furnace with hydrogen as carrier gas to form a strip catalyst.

[0012] Preferably, the MXene precursor MAX is Ti4AlN3, Ti2AlC, TiNbAlC, Ti3AlC, Ta4AlC3, Nb2AlC, V2AlC, Nb4AlC3, Mo2AlC, (Nb 0.8 Ti 0.2 )4AlC3、(Nb 0.8 Zr 0.2 )Any one of 4AlC3, Zr3AlC2 or Hf3AlC2.

[0013] Preferably, the molar ratio of concentrated hydrochloric acid to lithium fluoride in the mixed solution of concentrated hydrochloric acid and lithium fluoride is (1-6):1.

[0014] Preferably, the volume of the mixed solution of concentrated hydrochloric acid and lithium fluoride is 2-10 times the mass of the MXene precursor MAX; in step (2), dicyandiamide accounts for 10-60wt% of the MXene; and the volume of ethanol accounts for 10-90% of the volume of the mixed solution of concentrated hydrochloric acid and lithium fluoride.

[0015] Preferably, the drying temperature is 80-120°C; the calcination conditions in step (2) are calcination at 300-650°C for 2-5h, and the calcination conditions in step (3) are calcination at 250-650°C for 2-5h; the reduction treatment conditions are reduction treatment at 180-600°C for 1-3h.

[0016] Preferably, in step (3), sodium hydroxide, potassium hydroxide, sodium carbonate, ammonia water or sodium bicarbonate is used to adjust the pH; the length of the strip catalyst is 4-7 mm and the diameter is 1.2-1.6 mm.

[0017] Preferably, in step (3), the hydrochloride or nitrate of the active metal M is used to prepare the aqueous solution of the active metal M.

[0018] The application of the catalyst in the continuous preparation of tris(hydroxymethyl)aminomethane is as follows: the catalyst is loaded into a reaction tube of a fixed bed reactor, the upper and lower sections of the reaction tube are filled with quartz sand, nitrogen is introduced into the fixed bed reactor at room temperature until the air in the fixed bed reactor is exhausted, and then hydrogen is introduced therein, the pressure is controlled at 0.8-1.5MPa, the temperature is increased to 50-70°C at a heating rate of 1.5-3°C / min and kept warm for 0.5-2h, and then the temperature is increased to a target reaction temperature of 110-150°C at a heating rate of 1-2°C / min and the temperature is maintained, the raw material tris(hydroxymethyl)nitromethane and the solvent are mixed and preheated to the target reaction temperature, and then pumped in through a high-pressure plunger pump, and hydrogen is kept continuously in and out; the solvent is one of methanol, ethanol, toluene, dichlorotoluene, tetrahydrofuran or isopropanol, the mass ratio of the raw material tris(hydroxymethyl)nitromethane to the solvent is 1:(2-10); the mass space velocity of the tris(hydroxymethyl)nitromethane is 0.1-0.35h -1 .

[0019] Preferably, the molar ratio of hydrogen to tris(hydroxymethyl)nitromethane is (15-65):1.

[0020] Advantages of the present invention:

[0021] (1) The catalyst of the present invention adopts a carrier MXene / C3N4 composed of MXene with a foam network structure coated with C3N4 capable of anchoring active metals. The catalyst prepared by using the carrier MXene / C3N4 to load active metals has very high catalytic activity and stability, and can achieve efficient catalytic preparation of tris(hydroxymethyl)aminomethane. The conversion rate of the raw material tris(hydroxymethyl)nitromethane is greater than 98%, and the yield of the product tris(hydroxymethyl)nitromethane is greater than 96%.

[0022] (2) The catalyst provided by the present invention realizes the continuous production of trishydroxyaminomethane, and can enable trishydroxymethylnitromethane to continuously prepare trishydroxymethylaminomethane. The reaction conditions are mild, the method is highly safe, the operating cost is low, it is easy to operate, it is green and controllable, and it has good market promotion prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 SEM image of carrier MXene / C3N4. DETAILED DESCRIPTION

[0024] Example 1

[0025] 1. A catalyst for synthesizing a sustained-release reagent for novel coronavirus detection, wherein the sustained-release reagent for novel coronavirus detection is tris(hydroxymethyl)aminomethane, and the catalyst is composed of a carrier MXene / C3N4 and an active metal Pd loaded on the carrier, wherein the loading amount of the active metal Pd is 0.5% by weight of the catalyst, and the remainder is the carrier;

[0026] 2. The method for preparing the catalyst for synthesizing the sustained-release reagent for novel coronavirus detection comprises the following steps:

[0027] (1) Preparation of MXene: 99.5 g of MXene precursor MAX (Ti4AlN3) was added to 200 mL of a mixed solution of concentrated hydrochloric acid and lithium fluoride with a molar ratio of 1:1, stirred at 600 r / min for 72 h, centrifuged and washed, liquid nitrogen was added to the precipitate, it was quickly frozen, and then placed in a vacuum freeze dryer until constant weight was obtained to obtain foamy MXene;

[0028] (2) Preparation of carrier MXene / C3N4: 30 g of dicyandiamide was dissolved in 95 mL of ethanol, 99.5 g of the MXene was added thereto, ultrasonically dispersed, stirred for 12 h, and then transferred to a hydrothermal reactor and kept at 150 °C for 12 h. The filter cake was taken out and dried in an oven at 120 °C to constant weight, and then calcined in a muffle furnace at 650 °C for 3 h to obtain a carrier MXene / C3N4 with a C3N4-coated MXene foam network structure. Figure 1 ;

[0029] (3) Preparation of catalyst: Using the equal volume impregnation method, take 5 mL of 0.1 g / mL palladium chloride active group solution, add deionized water to 150 g, adjust the pH to 2.5 with anhydrous sodium carbonate, add the carrier MXene / C3N4, stir evenly, impregnate for 12 h, dry at 120 ° C to constant weight, calcine in a muffle furnace at 500 ° C for 3 h, and then reduce in a tubular furnace with hydrogen as carrier gas at 300 ° C for 2 h to obtain a powdered catalyst. The powdered catalyst is molded into a strip catalyst by an extruder. The strip catalyst has a length of 4-7 mm and a diameter of 1.2-1.6 mm.

[0030] Example 2

[0031] 1. A catalyst for synthesizing a sustained-release reagent for novel coronavirus detection, wherein the sustained-release reagent for novel coronavirus detection is tris(hydroxymethyl)aminomethane, and the catalyst is composed of a carrier MXene / C3N4 and an active metal Pt loaded on the carrier, wherein the loading amount of the active metal Pt is 0.5% by weight of the catalyst, and the remainder is the carrier;

[0032] 2. The method for preparing the catalyst for synthesizing the sustained-release reagent for novel coronavirus detection comprises the following steps:

[0033] (1) Preparation of MXene: 99.5 g of MXene precursor MAX (Ti4AlN3) was added to 200 mL of a mixed solution of concentrated hydrochloric acid and lithium fluoride with a molar ratio of 1:1, stirred at 600 r / min for 72 h, centrifuged and washed, liquid nitrogen was added to the precipitate, it was quickly frozen, and then placed in a vacuum freeze dryer until constant weight was obtained to obtain foamy MXene;

[0034] (2) Preparation of carrier MXene / C3N4: 30 g of dicyandiamide was dissolved in 105 mL of ethanol, 99.5 g of the MXene was added thereto, ultrasonically dispersed, stirred for 15 h, and then transferred to a hydrothermal reactor and kept at 175 °C for 15 h. The filter cake was taken out and dried in an oven at 120 °C to constant weight, and then calcined in a muffle furnace at 560 °C for 3 h to obtain a carrier MXene / C3N4 with a C3N4-coated MXene foam network structure;

[0035] (3) Preparation of catalyst: Using the equal volume impregnation method, take 5 mL of 0.1 g / mL platinum chloride active group solution, add deionized water to 150 g, adjust the pH to 2.1 with anhydrous sodium carbonate, add the carrier MXene / C3N4, stir evenly, impregnate for 12 h, dry at 120 ° C to constant weight, calcine in a muffle furnace at 450 ° C for 3 h, and then reduce in a tubular furnace with hydrogen as carrier gas at 300 ° C for 2 h to obtain a powdered catalyst. The powdered catalyst is molded into a strip catalyst by an extruder. The strip catalyst has a length of 4-7 mm and a diameter of 1.2-1.6 mm.

[0036] Example 3

[0037] 1. A catalyst for synthesizing a sustained-release reagent for novel coronavirus detection, wherein the sustained-release reagent for novel coronavirus detection is tris(hydroxymethyl)aminomethane, and the catalyst is composed of a carrier MXene / C3N4 and an active metal Rh loaded on the carrier, wherein the loading amount of the active metal Rh is 0.5% by weight of the catalyst, and the remainder is the carrier;

[0038] 2. The method for preparing the catalyst for synthesizing the sustained-release reagent for novel coronavirus detection comprises the following steps:

[0039] (1) Preparation of MXene: 99.5 g of MXene precursor MAX (Ti4AlN3) was added to 200 mL of a mixed solution of concentrated hydrochloric acid and lithium fluoride with a molar ratio of 1:1, stirred at 600 r / min for 72 h, centrifuged and washed, liquid nitrogen was added to the precipitate, it was quickly frozen, and then placed in a vacuum freeze dryer until constant weight was obtained to obtain foamy MXene;

[0040] (2) Preparation of carrier MXene / C3N4: 30 g of dicyandiamide was dissolved in 100 mL of ethanol, 99.5 g of the MXene was added thereto, ultrasonically dispersed, stirred for 16 h, and then transferred to a hydrothermal reactor and kept at 180 °C for 16 h. The filter cake was taken out and dried in an oven at 120 °C to constant weight, and then calcined in a muffle furnace at 400 °C for 3 h to obtain a carrier MXene / C3N4 with a C3N4-coated MXene foam network structure;

[0041] (3) Preparation of catalyst: Using the equal volume impregnation method, take 5 mL of 0.1 g / mL rhodium trichloride active group solution, add deionized water to 150 g, adjust the pH to 2.8 with anhydrous sodium carbonate, add the carrier MXene / C3N4 thereto, stir evenly, impregnate for 12 h, dry at 120 ° C to constant weight, calcine in a muffle furnace at 350 ° C for 3 h, and then reduce in a tubular furnace with hydrogen as carrier gas at 260 ° C for 2 h to obtain a powdered catalyst, and shape the powdered catalyst into a strip catalyst by an extruder. The strip catalyst has a length of 4-7 mm and a diameter of 1.2-1.6 mm.

[0042] Example 4

[0043] 1. A catalyst for synthesizing a sustained-release reagent for novel coronavirus detection, wherein the sustained-release reagent for novel coronavirus detection is tris(hydroxymethyl)aminomethane, and the catalyst is composed of a carrier MXene / C3N4 and an active metal Ru loaded on the carrier, wherein the loading amount of the active metal Ru is 0.5% by weight of the catalyst, and the remainder is the carrier;

[0044] 2. The method for preparing the catalyst for synthesizing the sustained-release reagent for novel coronavirus detection comprises the following steps:

[0045] (1) Preparation of MXene: 99.5 g of MXene precursor MAX (Ti4AlN3) was added to 200 mL of a mixed solution of concentrated hydrochloric acid and lithium fluoride with a molar ratio of 1:1, stirred at 600 r / min for 72 h, centrifuged and washed, liquid nitrogen was added to the precipitate, it was quickly frozen, and then placed in a vacuum freeze dryer until constant weight was obtained to obtain foamy MXene;

[0046] (2) Preparation of carrier MXene / C3N4: 30 g of dicyandiamide was dissolved in 100 mL of ethanol, 99.5 g of the MXene was added thereto, ultrasonically dispersed, stirred for 22 h, and then transferred to a hydrothermal reactor and kept at 175 °C for 24 h. The filter cake was taken out and dried in an oven at 120 °C to constant weight, and then calcined in a muffle furnace at 350 °C for 3 h to obtain a carrier MXene / C3N4 with a C3N4-coated MXene foam network structure;

[0047] (3) Preparation of catalyst: Using the equal volume impregnation method, take 5 mL of 0.1 g / mL ruthenium trichloride active group solution, add deionized water to 150 g, adjust the pH to 2.0 with anhydrous sodium carbonate, add the carrier MXene / C3N4 thereto, stir evenly, impregnate for 12 hours, dry at 120°C to constant weight, calcine in a muffle furnace at 500°C for 3 hours, and then reduce in a tubular furnace at 200°C for 2 hours with hydrogen as carrier gas to obtain a powdered catalyst. The powdered catalyst is molded into a strip catalyst by an extruder. The strip catalyst has a length of 4-7 mm and a diameter of 1.2-1.6 mm.

[0048] Example 5

[0049] 1. A catalyst for synthesizing a sustained-release reagent for novel coronavirus detection, wherein the sustained-release reagent for novel coronavirus detection is tris(hydroxymethyl)aminomethane, and the catalyst is composed of a carrier MXene / C3N4 and an active metal Ni loaded on the carrier, wherein the loading amount of the active metal Ni is 5% by weight of the catalyst, and the remainder is the carrier;

[0050] 2. The method for preparing the catalyst for synthesizing the sustained-release reagent for novel coronavirus detection comprises the following steps:

[0051] (1) Preparation of MXene: 99.5 g of MXene precursor MAX (Ti4AlN3) was added to 200 mL of a mixed solution of concentrated hydrochloric acid and lithium fluoride with a molar ratio of 1:1, stirred at 600 r / min for 72 h, centrifuged and washed, liquid nitrogen was added to the precipitate, it was quickly frozen, and then placed in a vacuum freeze dryer until constant weight was obtained to obtain foamy MXene;

[0052] (2) Preparation of carrier MXene / C3N4: 30 g of dicyandiamide was dissolved in 120 mL of ethanol, 99.5 g of the MXene was added thereto, ultrasonically dispersed, stirred for 12 h, and then transferred to a hydrothermal reactor and kept at 180 °C for 12 h. The filter cake was taken out and dried in an oven at 120 °C to constant weight, and then calcined in a muffle furnace at 650 °C for 2 h to obtain a carrier MXene / C3N4 with a C3N4-coated MXene foam network structure;

[0053] (3) Preparation of catalyst: Using the equal volume impregnation method, take 24.7 g of nickel nitrate hexahydrate and add deionized water to 150 g, adjust the pH to 1.8 with anhydrous sodium carbonate, add the carrier MXene / C3N4, stir evenly, impregnate for 12 h, dry at 120 ° C to constant weight, calcine in a muffle furnace at 600 ° C for 2 h, and then reduce in a tubular furnace with hydrogen as carrier gas at 400 ° C for 2 h to obtain a powdered catalyst. The powdered catalyst is molded into a strip catalyst by an extruder. The strip catalyst has a length of 4-7 mm and a diameter of 1.2-1.6 mm.

[0054] Example 6

[0055] 1. A catalyst for synthesizing a sustained-release reagent for novel coronavirus detection, wherein the sustained-release reagent for novel coronavirus detection is tris(hydroxymethyl)aminomethane, and the catalyst is composed of a carrier MXene / C3N4 and an active metal Cu loaded on the carrier, wherein the loading amount of the active metal Cu is 5% by weight of the catalyst, and the remainder is the carrier;

[0056] 2. The method for preparing the catalyst for synthesizing the sustained-release reagent for novel coronavirus detection comprises the following steps:

[0057] (1) Preparation of MXene: 99.5 g of MXene precursor MAX (Ti4AlN3) was added to 200 mL of a mixed solution of concentrated hydrochloric acid and lithium fluoride with a molar ratio of 1:1, stirred at 600 r / min for 72 h, centrifuged and washed, liquid nitrogen was added to the precipitate, it was quickly frozen, and then placed in a vacuum freeze dryer until constant weight was obtained to obtain foamy MXene;

[0058] (2) Preparation of carrier MXene / C3N4: 30 g of dicyandiamide was dissolved in 80 mL of ethanol, 99.5 g of the MXene was added thereto, ultrasonically dispersed, stirred for 18 h, and then transferred to a hydrothermal reactor and kept at 215 °C for 18 h. The filter cake was taken out and dried in an oven at 120 °C to constant weight, and then calcined in a muffle furnace at 540 °C for 4 h to obtain a carrier MXene / C3N4 with a C3N4-coated MXene foam network structure;

[0059] (3) Preparation of catalyst: Using the equal volume impregnation method, 19.0 g of copper nitrate trihydrate was taken and deionized water was added to 150 g, the pH was adjusted to 3.0 with anhydrous sodium carbonate, and the carrier MXene / C3N4 was added thereto, stirred evenly, impregnated for 12 h, dried at 120 ° C to constant weight, calcined in a muffle furnace at 500 ° C for 5 h, and then reduced in a tubular furnace with hydrogen as carrier gas at 280 ° C for 2 h to obtain a powdered catalyst. The powdered catalyst was molded into a strip catalyst by an extruder. The strip catalyst had a length of 4-7 mm and a diameter of 1.2-1.6 mm.

[0060] Example 7

[0061] 1. A catalyst for synthesizing a sustained-release reagent for novel coronavirus detection, wherein the sustained-release reagent for novel coronavirus detection is tris(hydroxymethyl)aminomethane, and the catalyst is composed of a carrier MXene / C3N4 and an active metal Mg loaded on the carrier, wherein the loading amount of the active metal Mg is 5% by weight of the catalyst, and the remainder is the carrier;

[0062] 2. The method for preparing the catalyst for synthesizing the sustained-release reagent for novel coronavirus detection comprises the following steps:

[0063] (1) Preparation of MXene: 99.5 g of MXene precursor MAX (Ti4AlN3) was added to 200 mL of a mixed solution of concentrated hydrochloric acid and lithium fluoride with a molar ratio of 1:1, stirred at 600 r / min for 72 h, centrifuged and washed, liquid nitrogen was added to the precipitate, it was quickly frozen, and then placed in a vacuum freeze dryer until constant weight was obtained to obtain foamy MXene;

[0064] (2) Preparation of carrier MXene / C3N4: 30 g of dicyandiamide was dissolved in 68 mL of ethanol, 99.5 g of the MXene was added thereto, ultrasonically dispersed, stirred for 24 h, and then transferred to a hydrothermal reactor and kept at 165 °C for 36 h. The filter cake was taken out and dried in an oven at 120 °C to constant weight, and then calcined in a muffle furnace at 520 °C for 2.5 h to obtain a carrier MXene / C3N4 with a C3N4-coated MXene foam network structure;

[0065] (3) Preparation of catalyst: Using the equal volume impregnation method, 52.7 g of magnesium nitrate hexahydrate was taken and deionized water was added to 150 g, the pH was adjusted to 3.2 with anhydrous sodium carbonate, and the carrier MXene / C3N4 was added thereto, stirred evenly, impregnated for 12 h, dried at 120° C. to constant weight, calcined in a muffle furnace at 450° C. for 3.5 h, and then reduced in a tubular furnace at 400° C. for 2 h with hydrogen as carrier gas to obtain a powdered catalyst. The powdered catalyst was molded into a strip catalyst by an extruder, and the strip catalyst had a length of 4-7 mm and a diameter of 1.2-1.6 mm.

[0066] Example 8

[0067] 1. A catalyst for synthesizing a sustained-release reagent for novel coronavirus detection, wherein the sustained-release reagent for novel coronavirus detection is tris(hydroxymethyl)aminomethane, and the catalyst is composed of a carrier MXene / C3N4 and an active metal Co loaded on the carrier, wherein the loading amount of the active metal Co is 5% by weight of the catalyst, and the remainder is the carrier;

[0068] 2. The method for preparing the catalyst for synthesizing the sustained-release reagent for novel coronavirus detection comprises the following steps:

[0069] (1) Preparation of MXene: 99.5 g of MXene precursor MAX (Ti4AlN3) was added to 200 mL of a mixed solution of concentrated hydrochloric acid and lithium fluoride with a molar ratio of 1:1, stirred at 600 r / min for 72 h, centrifuged and washed, liquid nitrogen was added to the precipitate, it was quickly frozen, and then placed in a vacuum freeze dryer until constant weight was obtained to obtain foamy MXene;

[0070] (2) Preparation of carrier MXene / C3N4: 30 g of dicyandiamide was dissolved in 110 mL of ethanol, 99.5 g of the MXene was added thereto, ultrasonically dispersed, stirred for 16 h, and then transferred to a hydrothermal reactor and kept at 195 °C for 35 h. The filter cake was taken out and dried in an oven at 120 °C to constant weight, and then calcined in a muffle furnace at 600 °C for 5 h to obtain a carrier MXene / C3N4 with a C3N4-coated MXene foam network structure;

[0071] (3) Preparation of catalyst: Using the equal volume impregnation method, take 24.7 g of cobalt nitrate hexahydrate and add deionized water to 150 g, adjust the pH to 2.3 with anhydrous sodium carbonate, add the carrier MXene / C3N4, stir evenly, impregnate for 12 h, dry at 120 ° C to constant weight, calcine in a muffle furnace at 550 ° C for 2 h, and then reduce in a tubular furnace with hydrogen as carrier gas at 400 ° C for 2.5 h to obtain a powdered catalyst. The powdered catalyst is molded into a strip catalyst by an extruder. The strip catalyst has a length of 4-7 mm and a diameter of 1.2-1.6 mm.

[0072] Example 9

[0073] 1. A catalyst for synthesizing a sustained-release reagent for novel coronavirus detection, wherein the sustained-release reagent for novel coronavirus detection is tris(hydroxymethyl)aminomethane, and the catalyst is composed of a carrier MXene / C3N4 and an active metal Sn loaded on the carrier, wherein the loading amount of the active metal Sn is 5% by weight of the catalyst, and the balance is the carrier;

[0074] 2. The method for preparing the catalyst for synthesizing the sustained-release reagent for novel coronavirus detection comprises the following steps:

[0075] (1) Preparation of MXene: 99.5 g of MXene precursor MAX (Ti4AlN3) was added to 200 mL of a mixed solution of concentrated hydrochloric acid and lithium fluoride with a molar ratio of 1:1, stirred at 600 r / min for 72 h, centrifuged and washed, liquid nitrogen was added to the precipitate, it was quickly frozen, and then placed in a vacuum freeze dryer until constant weight was obtained to obtain foamy MXene;

[0076] (2) Preparation of carrier MXene / C3N4: 30 g of dicyandiamide was dissolved in 100 mL of ethanol, 99.5 g of the MXene was added thereto, ultrasonically dispersed, stirred for 24 h, and then transferred to a hydrothermal reactor and kept at 150 °C for 48 h. The filter cake was taken out and dried in an oven at 120 °C to constant weight, and then calcined in a muffle furnace at 350 °C for 3 h to obtain a carrier MXene / C3N4 with a C3N4-coated MXene foam network structure;

[0077] (3) Preparation of catalyst: Using the equal volume impregnation method, take 7.9 g of stannous chloride and add dilute hydrochloric acid to 150 g, adjust the pH to 1.9 with anhydrous sodium carbonate, add the carrier MXene / C3N4, stir evenly, impregnate for 12 h, dry at 120 ° C to constant weight, calcine in a muffle furnace at 480 ° C for 4 h, and then reduce in a tubular furnace with hydrogen as carrier gas at 260 ° C for 2 h to obtain a powdered catalyst. The powdered catalyst is formed into a strip catalyst by an extruder. The strip catalyst has a length of 4-7 mm and a diameter of 1.2-1.6 mm.

[0078] Example 10

[0079] 1. A catalyst for synthesizing a sustained-release reagent for novel coronavirus detection, wherein the sustained-release reagent for novel coronavirus detection is tris(hydroxymethyl)aminomethane, and the catalyst is composed of a carrier MXene / C3N4 and an active metal Fe loaded on the carrier, wherein the loading amount of the active metal Fe is 5% by weight of the catalyst, and the remainder is the carrier;

[0080] 2. The method for preparing the catalyst for synthesizing the sustained-release reagent for novel coronavirus detection comprises the following steps:

[0081] (1) Preparation of MXene: 99.5 g of MXene precursor MAX (Ti4AlN3) was added to 200 mL of a mixed solution of concentrated hydrochloric acid and lithium fluoride with a molar ratio of 1:1, stirred at 600 r / min for 48 h, centrifuged and washed, liquid nitrogen was added to the precipitate, which was quickly frozen and then placed in a vacuum freeze dryer until constant weight was obtained to obtain foamy MXene;

[0082] (2) Preparation of carrier MXene / C3N4: 30 g of dicyandiamide was dissolved in 80 mL of ethanol, 99.5 g of the MXene was added thereto, ultrasonically dispersed, stirred for 18 h, and then transferred to a hydrothermal reactor and kept at 175 °C for 20 h. The filter cake was taken out and dried in an oven at 120 °C to constant weight, and then calcined in a muffle furnace at 600 °C for 2 h to obtain a carrier MXene / C3N4 with a C3N4-coated MXene foam network structure;

[0083] (3) Preparation of catalyst: Using the equal volume impregnation method, take 24.2 g of ferric chloride hexahydrate and add deionized water to 150 g, adjust the pH to 2.6 with anhydrous sodium carbonate, add the carrier MXene / C3N4 thereto, stir evenly, impregnate for 12 hours, dry at 120°C to constant weight, calcine in a muffle furnace at 450°C for 3 hours, and then reduce in a tubular furnace at 350°C for 2 hours with hydrogen as carrier gas to obtain a powdered catalyst. The powdered catalyst is molded into a strip catalyst by an extruder. The strip catalyst has a length of 4-7 mm and a diameter of 1.2-1.6 mm.

[0084] Embodiment 11

[0085] 1. A catalyst for synthesizing a sustained-release reagent for novel coronavirus detection, wherein the sustained-release reagent for novel coronavirus detection is tris(hydroxymethyl)aminomethane, and the catalyst is composed of a carrier MXene / C3N4 and an active metal Mn loaded on the carrier, wherein the loading amount of the active metal Mn is 5% by weight of the catalyst, and the balance is the carrier;

[0086] 2. The method for preparing the catalyst for synthesizing the sustained-release reagent for novel coronavirus detection comprises the following steps:

[0087] (1) Preparation of MXene: 99.5 g of MXene precursor MAX (Ti4AlN3) was added to 200 mL of a mixed solution of concentrated hydrochloric acid and lithium fluoride with a molar ratio of 1:1, stirred at 600 r / min for 48 h, centrifuged and washed, liquid nitrogen was added to the precipitate, which was quickly frozen and then placed in a vacuum freeze dryer until constant weight was obtained to obtain foamy MXene;

[0088] (2) Preparation of carrier MXene / C3N4: 30 g of dicyandiamide was dissolved in 90 mL of ethanol, 99.5 g of the MXene was added thereto, ultrasonically dispersed, stirred for 16.5 h, and then transferred to a hydrothermal reactor and kept at 170 °C for 12 h. The filter cake was taken out and dried in an oven at 120 °C to constant weight, and then calcined in a muffle furnace at 650 °C for 3 h to obtain a carrier MXene / C3N4 with a C3N4-coated MXene foam network structure;

[0089] (3) Preparation of catalyst: Using the equal volume impregnation method, take 26.1 g of manganese nitrate hexahydrate and add deionized water to 150 g, adjust the pH to 2.2 with anhydrous sodium carbonate, add the carrier MXene / C3N4, stir evenly, impregnate for 12 h, dry at 120 ° C to constant weight, calcine in a muffle furnace at 400 ° C for 3 h, and then reduce in a tubular furnace with hydrogen as carrier gas at 260 ° C for 2 h to obtain a powdered catalyst. The powdered catalyst is molded into a strip catalyst by an extruder. The strip catalyst has a length of 4-7 mm and a diameter of 1.2-1.6 mm.

[0090] Example 12

[0091] 1. A catalyst for synthesizing a sustained-release reagent for novel coronavirus detection, wherein the sustained-release reagent for novel coronavirus detection is tris(hydroxymethyl)aminomethane, and the catalyst is composed of a carrier MXene / C3N4 and an active metal La loaded on the carrier, wherein the loading amount of the active metal La is 5% by weight of the catalyst, and the remainder is the carrier;

[0092] 2. The method for preparing the catalyst for synthesizing the sustained-release reagent for novel coronavirus detection comprises the following steps:

[0093] (1) Preparation of MXene: 99.5 g of MXene precursor MAX (Ti4AlN3) was added to 200 mL of a mixed solution of concentrated hydrochloric acid and lithium fluoride with a molar ratio of 1:1, stirred at 600 r / min for 72 h, centrifuged and washed, liquid nitrogen was added to the precipitate, it was quickly frozen, and then placed in a vacuum freeze dryer until constant weight was obtained to obtain foamy MXene;

[0094] (2) Preparation of carrier MXene / C3N4: 30 g of dicyandiamide was dissolved in 70 mL of ethanol, 99.5 g of the MXene was added thereto, ultrasonically dispersed, stirred for 12 h, and then transferred to a hydrothermal reactor and kept at 225 °C for 48 h. The filter cake was taken out and dried in an oven at 120 °C to constant weight, and then calcined in a muffle furnace at 350 °C for 2 h to obtain a carrier MXene / C3N4 with a C3N4-coated MXene foam network structure;

[0095] (3) Preparation of catalyst: Using the equal volume impregnation method, take 15.6 g of lanthanum nitrate hexahydrate and add deionized water to 150 g, adjust the pH to 3.4 with anhydrous sodium carbonate, add the carrier MXene / C3N4, stir evenly, impregnate for 12 hours, dry at 120°C to constant weight, calcine in a muffle furnace at 300°C for 3 hours, and then reduce in a tubular furnace at 250°C for 2 hours with hydrogen as carrier gas to obtain a powdered catalyst. The powdered catalyst is molded into a strip catalyst by an extruder. The strip catalyst has a length of 4-7 mm and a diameter of 1.2-1.6 mm.

[0096] Example 13

[0097] 1. A catalyst for synthesizing a sustained-release reagent for novel coronavirus detection, wherein the sustained-release reagent for novel coronavirus detection is tris(hydroxymethyl)aminomethane, and the catalyst is composed of a carrier MXene / C3N4 and an active metal Pd loaded on the carrier, wherein the loading amount of the active metal Pd is 0.3% by weight of the catalyst, and the remainder is the carrier;

[0098] 2. The method for preparing the catalyst for synthesizing the sustained-release reagent for novel coronavirus detection comprises the following steps:

[0099] (1) Preparation of MXene: 99.5 g of MXene precursor MAX (Ti2AlC) was added to 995 mL of a mixed solution of concentrated hydrochloric acid and lithium fluoride with a molar ratio of 6:1, stirred at 300 r / min for 36 h, centrifuged and washed, liquid nitrogen was added to the precipitate, quickly frozen, and then placed in a vacuum freeze dryer until constant weight was obtained to obtain foamy MXene;

[0100] (2) Preparation of carrier MXene / C3N4: 10 g of dicyandiamide was dissolved in 200 mL of ethanol, 99.5 g of the MXene was added thereto, ultrasonically dispersed, stirred for 36 h, and then transferred to a hydrothermal reactor and kept at 225 °C for 12 h. The filter cake was taken out and dried in an oven at 80 °C to constant weight, and then calcined in a muffle furnace at 300 °C for 5 h to obtain a carrier MXene / C3N4 with a C3N4-coated MXene foam network structure;

[0101] (3) Preparation of catalyst: Using the equal volume impregnation method, take 5 mL of 0.1 g / mL palladium chloride active group solution, add deionized water to 150 g, adjust the pH to 3.6 with anhydrous sodium carbonate, add the carrier MXene / C3N4, stir evenly, impregnate for 36 hours, dry at 80°C to constant weight, calcine in a muffle furnace at 250°C for 5 hours, and then reduce in a tubular furnace at 180°C for 3 hours with hydrogen as carrier gas to obtain a powdered catalyst. The powdered catalyst is molded into a strip catalyst by an extruder. The strip catalyst has a length of 4-7 mm and a diameter of 1.2-1.6 mm.

[0102] Embodiment 14

[0103] 1. A catalyst for synthesizing a sustained-release reagent for novel coronavirus detection, wherein the sustained-release reagent for novel coronavirus detection is tris(hydroxymethyl)aminomethane, and the catalyst is composed of a carrier MXene / C3N4 and an active metal Pd loaded on the carrier, wherein the loading amount of the active metal Pd is 0.7% by weight of the catalyst, and the remainder is the carrier;

[0104] 2. The method for preparing the catalyst for synthesizing the sustained-release reagent for novel coronavirus detection comprises the following steps:

[0105] (1) Preparation of MXene: 99.5 g of MXene precursor MAX (TiNbAlC) was added to 995 mL of a mixed solution of concentrated hydrochloric acid and lithium fluoride with a molar ratio of 6:1, stirred at 300 r / min for 36 h, centrifuged and washed, liquid nitrogen was added to the precipitate, it was quickly frozen, and then placed in a vacuum freeze dryer until constant weight was obtained to obtain foamy MXene;

[0106] (2) Preparation of carrier MXene / C3N4: 59.7 g of dicyandiamide was dissolved in 335 mL of ethanol, 99.5 g of the MXene was added thereto, ultrasonically dispersed, stirred for 36 h, and then transferred to a hydrothermal reactor and kept at 225 °C for 12 h. The filter cake was taken out and dried in an oven at 80 °C to constant weight, and then calcined in a muffle furnace at 300 °C for 5 h to obtain a carrier MXene / C3N4 with a C3N4-coated MXene foam network structure;

[0107] (3) Preparation of catalyst: Using the equal volume impregnation method, take 5 mL of 0.1 g / mL palladium chloride active group solution, add deionized water to 150 g, adjust the pH to 3.6 with anhydrous sodium carbonate, add the carrier MXene / C3N4, stir evenly, impregnate for 36 hours, dry at 80°C to constant weight, calcine at 650°C in a muffle furnace for 2 hours, and then reduce in a tubular furnace with hydrogen as carrier gas at 600°C for 1 hour to obtain a powdered catalyst. The powdered catalyst is molded into a strip catalyst by an extruder. The strip catalyst has a length of 4-7 mm and a diameter of 1.2-1.6 mm.

[0108] Embodiment 15

[0109] 1. A catalyst for synthesizing a sustained-release reagent for novel coronavirus detection, wherein the sustained-release reagent for novel coronavirus detection is tris(hydroxymethyl)aminomethane, and the catalyst is composed of a carrier MXene / C3N4 and an active metal La loaded on the carrier, wherein the loading amount of the active metal La is 0.5% by weight of the catalyst, and the remainder is the carrier;

[0110] 2. The method for preparing the catalyst for synthesizing the sustained-release reagent for novel coronavirus detection comprises the following steps:

[0111] (1) Preparation of MXene: 99.5 g of MXene precursor MAX (TiNbAlC) was added to 995 mL of a mixed solution of concentrated hydrochloric acid and lithium fluoride with a molar ratio of 6:1, stirred at 300 r / min for 36 h, centrifuged and washed, liquid nitrogen was added to the precipitate, it was quickly frozen, and then placed in a vacuum freeze dryer until constant weight was obtained to obtain foamy MXene;

[0112] (2) Preparation of carrier MXene / C3N4: 59.7 g of dicyandiamide was dissolved in 400 mL of ethanol, 99.5 g of the MXene was added thereto, ultrasonically dispersed, stirred for 36 h, and then transferred to a hydrothermal reactor and kept at 225 °C for 12 h. The filter cake was taken out and dried in an oven at 80 °C to constant weight, and then calcined in a muffle furnace at 300 °C for 5 h to obtain a carrier MXene / C3N4 with a C3N4-coated MXene foam network structure;

[0113] (3) Preparation of catalyst: Using the equal volume impregnation method, take 15.6 g of lanthanum nitrate hexahydrate and add deionized water to 150 g, adjust the pH to 3.6 with anhydrous sodium carbonate, add the carrier MXene / C3N4, stir evenly, impregnate for 36 hours, dry at 80°C to constant weight, calcine at 650°C in a muffle furnace for 2 hours, and then reduce in a tubular furnace with hydrogen as carrier gas at 600°C for 1 hour to obtain a powdered catalyst. The powdered catalyst is molded into a strip catalyst by an extruder. The strip catalyst has a length of 4-7 mm and a diameter of 1.2-1.6 mm.

[0114] Example 16

[0115] The loading amount of La is 10%, and the rest is the same as Example 15.

[0116] Embodiment 17

[0117] The loading amount of La is 0.2%, and the rest is the same as Example 15.

[0118] Embodiment 18

[0119] The loading amount of Pd is 0.2%, and the rest is the same as in Example 1.

[0120] Embodiment 19

[0121] The loading amount of Pd is 1%, and the others are the same as in Example 1.

[0122] Comparative Example 1

[0123] When preparing the catalyst, melamine is used instead of dicyandiamide in step (2), and the rest is the same as in Example 1.

[0124] Embodiment 20

[0125] The catalyst provided by the present invention is used to continuously prepare tris(hydroxymethyl)aminomethane, specifically as follows: the catalyst is loaded into a reaction tube of a fixed bed reactor, the upper and lower sections of the reaction tube are filled with quartz sand, nitrogen is introduced into the fixed bed reactor at room temperature until the air in the fixed bed reactor is exhausted, and then hydrogen is introduced therein, the pressure is controlled at 1.0 MPa, the temperature is increased to 60°C at a heating rate of 1.6°C / min and kept warm for 2h, and then the temperature is increased to a target reaction temperature of 120°C at a heating rate of 1.5°C / min and the temperature is maintained, the raw material tris(hydroxymethyl)nitromethane and the solvent methanol are mixed in a mass ratio of 1:5 and preheated to the target reaction temperature, and then pumped in by a high-pressure plunger pump, the molar ratio of hydrogen to tris(hydroxymethyl)nitromethane is 30:1 and continuous inflow and outflow are maintained; the mass space velocity of the tris(hydroxymethyl)nitromethane is 0.25h -1 .

[0126] The reaction results are shown in Table 1.

[0127] Table 1 Reaction results of continuous preparation of tris(hydroxymethyl)aminomethane

[0128]

Claims

1. A catalyst for synthesizing a sustained-release reagent for novel coronavirus detection, wherein the sustained-release reagent for novel coronavirus detection is tris(hydroxymethyl)aminomethane, Features: The catalyst is composed of a carrier and an active metal loaded on the carrier, wherein the active metal is a noble metal M 1 Or non-precious metal M 2 , the carrier is MXene / C 3 N 4 , the noble metal M 1 is Pd, Pt, Rh or Ru, the non-precious metal M 2 is Cu, Fe, Ni, Mn, Co, Mg, La or Sn; in terms of weight ratio of the catalyst, the noble metal M 1 The loading amount is 0.2%-1%, and the non-precious metal M 2 The loading amount is 0.2%-10%, and the balance is the carrier; The catalyst for synthesizing a sustained-release reagent for novel coronavirus detection comprises the following steps: (1) Preparation of MXene: Take the MXene precursor MAX and add it to a mixed solution of concentrated hydrochloric acid and lithium fluoride, stir for 36-72 hours, centrifuge and wash, add liquid nitrogen to the precipitate, freeze it quickly, and then place it in a vacuum freeze dryer until constant weight is obtained to obtain foamy MXene; (2) Carrier MXene / C 3 N 4 Preparation: Dissolve dicyandiamide in ethanol, add the MXene thereto, disperse by ultrasonication, stir for 12-36 hours, keep at 150-225°C for 12-48 hours, take out and filter, dry the filter cake to constant weight, and then calcine to obtain C 3 N 4 MXene / C, a carrier with a network structure coated with MXene foam 3 N 4 ; (3) Preparation of catalyst: Prepare an aqueous solution of active metal M by equal volume impregnation method, adjust the pH to 1.8-3.6, and add the carrier MXene / C 3 N 4 , stir evenly, soak for 12-36 hours, dry to constant weight, calcine, and then reduce in a tubular furnace with hydrogen as carrier gas to form a strip catalyst.

2. A catalyst for synthesizing a sustained-release reagent for novel coronavirus detection according to claim 1, Features: The precious metal M 1 The loading amount is 0.3%-0.7%, and the non-precious metal M 2 The loading amount is 0.5%-5%.

3. A catalyst for synthesizing a sustained-release reagent for novel coronavirus detection according to claim 1, Features: The MXene precursor MAX is Ti 4 AlN 3 、Ti 2 AlC, TiNbAlC, Ti 3 AlC、Ta 4 AlC 3 , Nb 2 AlC、V 2 AlC、Nb 4 AlC 3 、Mo 2 AlC, (Nb 0.8 Ti 0.2 ) 4 AlC 3 、(Nb 0.8 Zr 0.2 ) 4 AlC 3 、Zr 3 AlC 2 or Hf 3 AlC 2 Any one of .

4. A catalyst for synthesizing a sustained-release reagent for novel coronavirus detection according to claim 1, Features: The molar ratio of concentrated hydrochloric acid to lithium fluoride in the concentrated hydrochloric acid and lithium fluoride mixed solution is (1-6):

1.

5. A catalyst for synthesizing a sustained-release reagent for novel coronavirus detection according to claim 1, Features: The volume of the mixed solution of concentrated hydrochloric acid and lithium fluoride is 2-10 times the mass of the MXene precursor MAX; in step (2), dicyandiamide accounts for 10-60wt% of the MXene; and the volume of ethanol accounts for 10-90% of the volume of the mixed solution of concentrated hydrochloric acid and lithium fluoride.

6. A catalyst for synthesizing a sustained-release reagent for novel coronavirus detection according to claim 1, Features: The drying temperature is 80-120°C; the calcination conditions in step (2) are calcination at 300-650°C for 2-5h, and the calcination conditions in step (3) are calcination at 250-650°C for 2-5h; the reduction treatment conditions are reduction treatment at 180-600°C for 1-3h.

7. A catalyst for synthesizing a sustained-release reagent for novel coronavirus detection according to claim 1, Features: In step (3), the pH is adjusted using sodium hydroxide, potassium hydroxide, sodium carbonate, ammonia water or sodium bicarbonate; The strip catalyst has a length of 4-7 mm and a diameter of 1.2-1.6 mm.

8. Use of the catalyst according to claim 1 in the continuous preparation of tris(hydroxymethyl)aminomethane, Features: Specifically, the catalyst is loaded into a reaction tube of a fixed bed reactor, the upper and lower sections of the reaction tube are filled with quartz sand, nitrogen is introduced into the fixed bed reactor at room temperature until the air in the fixed bed reactor is exhausted, and then hydrogen is introduced therein, the pressure is controlled at 0.8-1.5MPa, the temperature is increased to 50-70°C at a heating rate of 1.5-3°C / min and kept warm for 0.5-2h, and then the temperature is increased to the target reaction temperature of 110-150°C at a heating rate of 1-2°C / min and the temperature is maintained, the raw material trimethylolnitromethane and the solvent are mixed and preheated to the target reaction temperature, and then pumped in through a high-pressure plunger pump, and hydrogen is kept continuously in and out; the solvent is one of methanol, ethanol, toluene, dichlorotoluene, tetrahydrofuran or isopropanol, the mass ratio of the raw material trimethylolnitromethane to the solvent is 1:(2-10); the mass space velocity of the trimethylolnitromethane is 0.1-0.35h -1 .

9. Use of the catalyst according to claim 8 in the continuous preparation of tris(hydroxymethyl)aminomethane, Features: The molar ratio of hydrogen to trimethylolnitromethane is (15-65):1.