A method for preparing color-changing polyurea
By uniformly distributing color-changing groups on the main chain of the polyurea molecule, a four-step reaction is used to prepare force-photochromic polyurea, which solves the problem of poor performance of existing photochromic materials and achieves high stability and good physical and mechanical properties. , extending the service life of the material.
Patent Information
- Application Number
- CN202211557627.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-06
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-12-06
AI Technical Summary
Existing photochromic polyurea materials have poor performance and insufficient thermal stability and fatigue resistance. The combination form and amount of photochromic materials and polyurea determine the discoloration effect of the material, but they lack force-chromic function.
By introducing color-changing groups into the main chain of the polyurea molecule, each polyurea segment is evenly distributed with color-changing groups, and a four-step reaction is used to prepare force-photochromic polyurea. The reaction does not contain polyols and urethane bonds, only urea bonds, avoiding catalysts and ensuring material stability and performance.
It achieves high stability and good physical and mechanical properties of polyurea materials. The discoloration groups are evenly distributed and sensitive to external stimulation. It extends the long-term discoloration performance and service life of the material and solves the problems of poor thermal stability and fatigue resistance.
Smart Images

Figure BDA0003983291920000051 
Figure BDA0003983291920000061 
Figure FHA0000006839430000021
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, in particular to a method for preparing color-changing polyurea. Background Art
[0002] In recent years, photochromic materials have attracted more and more attention due to their extremely high potential application value and have become an important research topic internationally. Photochromic materials have not only been put into practical use in the fields of photosensitive decoration, color-changing glasses, digital display, etc., but also have very attractive prospects in high-tech fields such as optical information storage, optical switches, holographic ultrafine development, and biological probes. Under the action of an external force field, mechanochromic materials can qualitatively judge the stress state of the material through the change of material color and color distribution. Therefore, the color change phenomenon can be used to study polymers at the molecular level.
[0003] Polyurea is an elastomeric substance generated by the reaction of isocyanate components and amino compound components. Due to the high bond energy of urea bonds, polyurea has excellent mechanical properties, such as high strength, high wear resistance, high impact resistance, excellent flexibility, and excellent weather resistance and chemical resistance. It is widely used in pipelines, construction, energy, transportation, water conservancy, chemical industry, military and other anti-corrosion protection fields.
[0004] Therefore, if the functional advantages of the two can be combined to achieve force-photochromic polyurea, the advantages of the two can be combined and the material can be more widely used.
[0005] For example, Chinese patent CN110537114A discloses a method for producing photochromic eyeglass lenses. In an embodiment, at least one layer of improved photochromic poly(urea-urethane) is formed by combining a photochromic material and a polyurethane prepolymer with a reaction product of a mixture of diethyltoluenediamine and one or more polyols and a catalyst. The photochromic material is selected from at least one of silver halides, dichroic metal oxides, dichroic organic dyes, thermochromic compounds, spiro(indoline)pyrans, naphthopyrans, benzopyrans, dithizones, benzoxazines, spiro-oxazines, spiro(indoline)naphthooxazines, spiro-pyridobenzoxazines, anthraquinones, oxazines, indolizines, fulgides and fulgides.
[0006] However, the prior art achieves the photochromic effect of polyurea by adding photochromic materials. The raw materials of polyurea are common knowledge in the art. Isocyanate and polyol form prepolymers, and polyurethane prepolymers are combined with the reaction products of a mixture of diethyltoluenediamine and various polyols and a catalyst. The reaction product contains both urea bonds and urethane bonds. The urethane bonds have low reactivity and a tendency to foam. The material properties are poor. The system contains a catalyst and has poor durability.
[0007] Moreover, the above method for producing photochromic eyeglass lenses does not introduce how the photochromic material is combined with polyurea, i.e. physical mixing or chemical reaction? And the addition amount of the photochromic material is 0.25-2%. The combination form and addition amount of the photochromic material and polyurea determine the color change effect of the material. Again, the existing patent is only about photochromism, and does not mention mechanochromism. Summary of the invention
[0008] In view of this, the purpose of the present invention is to provide a method for preparing a color-changing polyurea. In the photochromic polyurea, the color-changing group is on the main chain of the polyurea molecule, which is an intrinsic functional group and each polyurea segment contains a color-changing group. The color-changing group is evenly distributed and is sensitive to external stimuli. The reaction does not involve polyols, and the corresponding product does not contain urethane bonds, only urea bonds, and the polymer is more stable and has better physical and mechanical properties.
[0009] To achieve the above object, the present invention provides the following technical solutions:
[0010] A method for preparing a color-changing polyurea comprises the following steps:
[0011] Step 1. Synthesis of Compound A
[0012] Weigh NR-4-chlorophenylhydrazine, 3-methyl-2-butanone and triethylamine raw materials by weight, add them into a three-necked flask in sequence, heat in a water bath and stir to react under nitrogen protection, then add sodium carbonate to neutralize, collect the fractions by distillation to obtain product a;
[0013] Step 2: Synthesis of compound b
[0014] In a round-bottom flask containing methanol solution, weighed compound a and 5-chlorosalicylaldehyde are added in sequence, a reflux condenser is installed, and the mixture is placed in an ultrasonic cleaner for water bath ultrasonic reflux reaction for 1-3 min, filtered, dried, and cooled to obtain compound b;
[0015] Step 3. Synthesis of compound c
[0016] Compound b was added to a round-bottom flask, and 10% ammonia methanol solution was added, and the mixture was placed in a water bath and stirred under reflux for 5-10 hours, and the excess solvent was distilled to obtain compound c;
[0017] Step 4. Synthesis of Compound d
[0018] Solid phosgene was dissolved in chloroform in a three-necked flask, and compound c was slowly added dropwise to the three-necked flask. The mixture was stirred and refluxed in a water bath for reaction. After the addition was completed, the excess solvent was distilled off to obtain compound d, a color-changing polyurea.
[0019] As a further embodiment of the present invention, in step 1, the three-necked flask is equipped with a stirrer, a thermometer and a reflux condenser device, and 2-6 parts of NR-4-chlorophenylhydrazine, 1-3 parts of 3-methyl-2-butanone and 1-3 parts of triethylamine are weighed by weight.
[0020] As a further scheme of the present invention, in step 1, under nitrogen protection, the reaction is heated in a water bath at 80°C and stirred, then neutralized with 1-3 parts of sodium carbonate, and the 240-320°C fraction is collected by distillation to obtain product a.
[0021] As a further embodiment of the present invention, the compound a is 1-5 parts of 5-chloro-1-R-group-3,3-dimethyl-2-methyleneindoline, wherein the R group of the compound a is benzene and its derivatives.
[0022] As a further scheme of the present invention, in step 2, 1-5 parts of compound a and 1-5 parts of 5-chlorosalicylaldehyde are added in sequence to a round-bottom flask containing 30 parts of methanol solution, a reflux condenser is installed, and the flask is placed in a 70W ultrasonic cleaner and ultrasonically refluxed at 70°C in a water bath for 1-3min.
[0023] As a further embodiment of the present invention, the purity of the 3-methyl-2-butanone and 5-chlorosalicylaldehyde is greater than or equal to 98%.
[0024] As a further embodiment of the present invention, in step 3, 1-5 parts of compound b are added to a round-bottom flask, and 10-50 parts of a 10% ammonia methanol solution are added, and the mixture is placed in a 70° C. water bath and stirred under reflux.
[0025] As a further solution of the present invention, in step 4, 0.5-1 parts of solid phosgene are dissolved in 50 parts of chloroform in a three-necked flask, 4-6 parts of compound c are slowly added dropwise to the three-necked flask, and the mixture is stirred and refluxed in a 70° C. water bath for reaction.
[0026] As a further embodiment of the present invention, the purity of the solid phosgene is ≥99.5%.
[0027] As a further embodiment of the present invention, the compound b is 5,6'-dichloro-1-benzyl-3,3-dimethylspiroindolinebenzopyran, and the compound c is 5,6'-diamino-1-benzyl-3,3-dimethylspiroindolinebenzopyran.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] The method for preparing a color-changing polyurea of the present invention prepares a photochromic polyurea, wherein the color-changing group is on the main chain of the polyurea molecule, is an intrinsic functional group, and each polyurea segment contains the color-changing group, the color-changing group is evenly distributed, and the color changes sensitively under external stimulation. The reaction does not involve polyols, the corresponding product does not contain urethane bonds, only urea bonds, the polymer is more stable, and the physical and mechanical properties are better.
[0030] 1. The method for preparing color-changing polyurea of the present invention comprises that each polyurea segment contains a color-changing group, the color-changing group is evenly distributed, and the color changes sensitively under external stimuli. The color-changing group changes color repeatedly, and the number of reversible cycles determines the long-term color-changing performance of the material. In the reversible process of CO bond breaking, a photochemical side reaction occurs, resulting in color-changing failure. The content of the color-changing group is high in the present application, which avoids the problem of color-changing failure of some color-changing groups.
[0031] 2. The polyurea polymer is obtained through a four-step reaction. Each molecular chain is connected by a urea bond. The reaction does not involve polyols. The corresponding product does not contain urethane bonds, but only urea bonds, which avoids the formation of bubbles when reacting with humid air. The polymer molecules are more stable and have better physical and mechanical properties. Moreover, the reaction does not require a catalyst, and there is no residual catalyst in the molecular chain. The material has good aging resistance and increases the service life of the material. The urea bond solves the shortcomings of photochromic materials such as poor thermal stability and poor fatigue resistance.
[0032] 3. The color-changing polyurea prepared by the present invention has readily available raw materials and low cost. DETAILED DESCRIPTION
[0033] The present invention is further described below in conjunction with specific embodiments. The specific implementation methods described below are intended to further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail, and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
[0034] The preparation method of the color-changing polyurea of the present application is used to prepare a force-photochromic polyurea. The color-changing group is on the main chain of the polyurea molecule and is an intrinsic functional group. The principle of force-photochromism is: when the colorless polymer molecule is irradiated with ultraviolet light or under force, the CO bond of the six-membered ring will undergo a reversible covalent bond break to generate an open ring body, so that it has strong absorption in the visible light region and produces color. Since the light response is reversible, the polymer can be reconnected to form a closed ring body when there is no light irradiation or force. The intrinsic functional group, the expression of force-photochromism is:
[0035]
[0036] A method for preparing a color-changing polyurea comprises the following steps:
[0037] Synthesis of compound a: In a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, add 2-6 parts of NR-4-chlorophenylhydrazine, then add 1-3 parts of 3-methyl-2-butanone and 1-3 parts of triethylamine, under nitrogen protection, heat in a water bath at 80°C and stir to react, then neutralize with 1-3 parts of sodium carbonate, and collect the 240-320°C fraction by distillation to obtain product a.
[0038] Synthesis of compound b: In a round-bottom flask containing 30 parts of methanol solution, add 1-5 parts of compound a and 1-5 parts of 5-chlorosalicylaldehyde in sequence, install a reflux condenser, place in a 70W ultrasonic cleaner, and react in a 70°C water bath for ultrasonic reflux reaction for 1-3 minutes, filter, dry, and cool to obtain compound b.
[0039] Synthesis of compound c: Add 1-5 parts of compound b into a round-bottom flask, add 10-50 parts of 10% ammonia methanol solution, place in a 70°C water bath, stir and reflux for 5-10 hours, and distill off excess solvent to obtain compound c.
[0040] Synthesis of compound d: Prepare 0.5-1 parts of solid phosgene in 50 parts of chloroform in a three-necked flask, slowly drop 4-6 parts of compound c into the three-necked flask, stir and reflux in a 70°C water bath to react, and after the dropwise addition is complete, distill the excess solvent to obtain compound d color-changing polyurea.
[0041] A method for preparing a color-changing polyurea is expressed as follows:
[0042]
[0043] Wherein, the compound a is 1-5 parts of 5-chloro-1-R-3,3-dimethyl-2-methyleneindoline, wherein the R group of compound a is benzene and its derivatives. The compound b is 5,6'-dichloro-1-benzyl-3,3-dimethylspiroindoline benzopyran, and the compound c is 5,6'-diamino-1-benzyl-3,3-dimethylspiroindoline benzopyran.
[0044] The technical solution of the present invention is further described in detail below in conjunction with specific implementation methods.
[0045] Example 1
[0046] The present invention provides a method for preparing a color-changing polyurea, and the synthesis process is as follows:
[0047] Synthesis of 5-chloro-1-phenyl-3,3-dimethyl-2-methyleneindoline: In a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, add 6 parts of N-phenyl-4-chlorophenylhydrazine, then add 3 parts of 3-methyl-2-butanone and 2 parts of triethylamine, and heat and stir the reaction in a water bath at 80°C under nitrogen protection, then neutralize with 2 parts of sodium carbonate, and collect the fraction at 200-280°C by distillation. The product 5-chloro-1-phenyl-3,3-dimethyl-2-methyleneindoline is obtained.
[0048] Synthesis of 5,6'-dichloro-1-phenyl-3,3-dimethylspiroindoline benzopyran: In a round-bottom flask containing 30 parts of methanol solution, 3 parts of 5-chloro-1-phenyl-3,3-dimethyl-2-methyleneindoline and 1 part of 5-chlorosalicylaldehyde were added in sequence, a reflux condenser was installed, and the mixture was placed in a 70W ultrasonic cleaner and subjected to ultrasonic reflux reaction at 70°C in a water bath for 3 min. The mixture was filtered, dried, and cooled to obtain 5,6'-dichloro-1-phenyl-3,3-dimethylspiroindoline benzopyran.
[0049] Synthesis of 5,6'-diamino-1-phenyl-3,3-dimethylspiroindoline benzopyran: 5 parts of 5,6'-dichloro-1-phenyl-3,3-dimethylspiroindoline benzopyran were added to a round-bottom flask, and 25 parts of 10% ammonia methanol solution were added, and the mixture was stirred and refluxed in a 70°C water bath for 10 hours, and the excess solvent was distilled to obtain 5,6'-diamino-1-phenyl-3,3-dimethylspiroindoline benzopyran. H NMR: m / z: 369.18 (100.0%), 370.19 (26.3%), 371.19 (3.5%), 370.18 (1.1%), elemental analysis: C, 78.02; H, 6.27; N, 11.37; O, 4.33.
[0050] Synthesis of color-changing polyurea: Prepare 1 part of solid phosgene and dissolve it in 50 parts of chloroform in a three-necked flask, slowly drop 5 parts of 5,6'-diamino-1-phenyl-3,3-dimethylspiroindolinebenzopyran into the three-necked flask, stir and reflux in a 70°C water bath to react, and after the dropwise addition is completed, distill the excess solvent to obtain the color-changing polyurea.
[0051] Secondly, using an ultraviolet spectrometer to test, the polyurea ultraviolet characteristic absorption peak is 565nm, the absorption peak intensity is 0.10, when illuminated, the absorption peak intensity is 0.85, an increase of 750%, when stretched 350%, the absorption peak intensity is 0.80, an increase of 700%, and there is obvious color change.
[0052] Example 2
[0053] The present invention provides a method for preparing a color-changing polyurea, and the synthesis process is as follows:
[0054] Synthesis of 5-chloro-1-benzyl-3,3-dimethyl-2-methyleneindoline: In a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, add 6 parts of N-benzyl-4-chlorophenylhydrazine, then add 2 parts of 3-methyl-2-butanone and 2 parts of triethylamine, and heat and stir the reaction in a water bath at 80°C under nitrogen protection, then neutralize with 2 parts of sodium carbonate, and collect the fraction at 220-300°C by distillation. The product 5-chloro-1-benzyl-3,3-dimethyl-2-methyleneindoline is obtained.
[0055] Synthesis of 5,6'-dichloro-1-benzyl-3,3-dimethylspiroindoline benzopyran: In a round-bottom flask containing 30 parts of methanol solution, 5 parts of 5-chloro-1-benzyl-3,3-dimethyl-2-methyleneindoline and 1 part of 5-chlorosalicylaldehyde were added in sequence, a reflux condenser was installed, and the mixture was placed in a 70W ultrasonic cleaner and subjected to ultrasonic reflux reaction at 70°C in a water bath for 3 min. The mixture was filtered, dried, and cooled to obtain 5,6'-dichloro-1-benzyl-3,3-dimethylspiroindoline benzopyran.
[0056] Synthesis of 5,6'-diamino-1-benzyl-3,3-dimethylspiroindoline benzopyran: 5 parts of 5,6'-dichloro-1-benzyl-3,3-dimethylspiroindoline benzopyran were added to a round-bottom flask, and 25 parts of 10% ammonia methanol solution were added, and the mixture was stirred and refluxed in a 70°C water bath for 10 hours, and the excess solvent was distilled to obtain 5,6'-diamino-1-benzyl-3,3-dimethylspiroindoline benzopyran. H NMR: m / z: m / z: 383.20 (100.0%), 384.20 (28.2%), 385.21 (3.6%), elemental analysis: C, 78.30; H, 6.57; N, 10.96; O, 4.17.
[0057] Synthesis of color-changing polyurea: Prepare 1 part of solid phosgene and dissolve it in 50 parts of chloroform in a three-necked flask, slowly drop 4 parts of 5,6'-diamino-1-phenyl-3,3-dimethylspiroindolinebenzopyran into the three-necked flask, stir and reflux in a 70°C water bath to react, and after the dropwise addition is completed, distill off the excess solvent to obtain the color-changing polyurea.
[0058] Secondly, using an ultraviolet spectrometer to test, the polyurea ultraviolet characteristic absorption peak is 565nm, the absorption peak intensity is 0.10, when illuminated, the absorption peak intensity is 0.85, an increase of 750%, when stretched 300%, the absorption peak intensity is 0.80, an increase of 700%, and there is obvious color change.
[0059] Example 3
[0060] The present invention provides a method for preparing a color-changing polyurea, and the synthesis process is as follows:
[0061] Synthesis of 5-chloro-1,3,3-trimethyl-2-methyleneindoline: In a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, add 6 parts of N-phenyl-4-chlorophenylhydrazine, then add 3 parts of 3-methyl-2-butanone and 2 parts of triethylamine, and heat and stir the reaction in a water bath at 80°C under nitrogen protection, then neutralize with 2 parts of sodium carbonate, and collect the fraction at 200-280°C by distillation. The product 5-chloro-1,3,3-trimethyl-2-methyleneindoline is obtained.
[0062] Synthesis of 5,6'-dichloro-1,3,3-trimethylspiroindoline benzopyran: In a round-bottom flask containing 30 parts of methanol solution, add 3 parts of 5-chloro-1,3,3-trimethyl-2-methyleneindoline and 1 part of 5-chlorosalicylaldehyde in sequence, install a reflux condenser, place in a 70W ultrasonic cleaner, and react in a 70℃ water bath for 3min of ultrasonic reflux reaction, filter, dry, and cool to obtain 5,6'-dichloro-1,3,3-trimethylspiroindoline benzopyran.
[0063] Synthesis of 5,6'-diamino-1,3,3-trimethylspiroindoline benzopyran: 5 parts of 5,6'-dichloro-1,3,3-trimethylspiroindoline benzopyran were added to a round-bottom flask, and 25 parts of 10% ammonia methanol solution were added, and the mixture was stirred and refluxed in a 70°C water bath for 10 hours, and the excess solvent was distilled to obtain 5,6'-diamino-1,3,3-trimethylspiroindoline benzopyran. H NMR: m / z: 307.17 (100.0%), 308.17 (21.9%), 309.18 (2.1%), elemental analysis: C, 74.24; H, 6.89; N, 13.67; O, 5.20.
[0064] Synthesis of polyurea: Prepare 1 part of solid phosgene and dissolve it in 50 parts of chloroform in a three-necked flask, slowly drop 5 parts of 5,6'-diamino-1,3,3-trimethylspiroindolinebenzopyran into the three-necked flask, stir and reflux in a 70°C water bath to react, and after the dropwise addition is completed, distill the excess solvent to obtain polyurea.
[0065] Secondly, the ultraviolet spectrometer was used for testing. The characteristic absorption peak of polyurea was 565nm, and the absorption peak intensity was 0.10. When exposed to light, the absorption peak intensity was 0.20, with an increase of 100%. When stretched 400%, the absorption peak intensity was 0.15, with an increase of 50%, and no color change. The tertiary amine of the spiro ring does not have the steric hindrance effect of the benzene ring, but reacts with phosgene to form a complex, destroying the color-changing group.
[0066] Comparative Example 1
[0067] This comparative example provides a method for synthesizing and preparing a polyurea material. Compared with Example 1, the R group uses a methyl group instead of a phenyl group. The synthesis and preparation process of the polyurea material is as follows:
[0068] Synthesis of 5-chloro-1,3,3-trimethyl-2-methyleneindoline: In a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, add 6 parts of N-phenyl-4-chlorophenylhydrazine, then add 3 parts of 3-methyl-2-butanone and 2 parts of triethylamine, and heat and stir the reaction in a water bath at 80°C under nitrogen protection, then neutralize with 2 parts of sodium carbonate, and collect the fraction at 200-280°C by distillation. The product 5-chloro-1,3,3-trimethyl-2-methyleneindoline is obtained.
[0069] Synthesis of 5,6'-dichloro-1,3,3-trimethylspiroindoline benzopyran: In a round-bottom flask containing 30 parts of methanol solution, add 3 parts of 5-chloro-1,3,3-trimethyl-2-methyleneindoline and 1 part of 5-chlorosalicylaldehyde in sequence, install a reflux condenser, place in a 70W ultrasonic cleaner, and react in a 70℃ water bath for 3min of ultrasonic reflux reaction, filter, dry, and cool to obtain 5,6'-dichloro-1,3,3-trimethylspiroindoline benzopyran.
[0070] Synthesis of 5,6'-diamino-1,3,3-trimethylspiroindoline benzopyran: 5 parts of 5,6'-dichloro-1,3,3-trimethylspiroindoline benzopyran were added to a round-bottom flask, and 25 parts of 10% ammonia methanol solution were added, and the mixture was stirred and refluxed in a 70°C water bath for 10 hours, and the excess solvent was distilled to obtain 5,6'-diamino-1,3,3-trimethylspiroindoline benzopyran. H NMR: m / z: 307.17 (100.0%), 308.17 (21.9%), 309.18 (2.1%), elemental analysis: C, 74.24; H, 6.89; N, 13.67; O, 5.20.
[0071] Synthesis of polyurea: Prepare 1 part of solid phosgene and dissolve it in 50 parts of chloroform in a three-necked flask, slowly drop 5 parts of 5,6'-diamino-1,3,3-trimethylspiroindolinebenzopyran into the three-necked flask, stir and reflux in a 70°C water bath to react, and after the dropwise addition is completed, distill the excess solvent to obtain polyurea.
[0072] Using an ultraviolet spectrometer to test, the characteristic ultraviolet absorption peak of polyurea is 565nm, the absorption peak intensity is 0.10, when illuminated, the absorption peak intensity is 0.20, the increase is 100%, when stretched 400%, the absorption peak intensity is 0.15, the increase is 50%, and there is no color change. The tertiary amine of the spiro ring does not have the steric hindrance effect of the benzene ring, but reacts with phosgene to form a complex, destroying the color-changing group.
[0073] Comparative Example 2
[0074] This comparative example provides a method for synthesizing and preparing a polyurea material. Compared with Example 1, the last step of the polyurea synthesis step is changed to dropwise adding solid phosgene into benzopyran. The synthesis and preparation process of the polyurea material is as follows:
[0075] Synthesis of 5-chloro-1-phenyl-3,3-dimethyl-2-methyleneindoline: In a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, add 6 parts of N-phenyl-4-chlorophenylhydrazine, then add 3 parts of 3-methyl-2-butanone and 2 parts of triethylamine, and heat and stir the reaction in a water bath at 80°C under nitrogen protection, then neutralize with 2 parts of sodium carbonate, and collect the fraction at 200-280°C by distillation. The product 5-chloro-1-phenyl-3,3-dimethyl-2-methyleneindoline is obtained.
[0076] Synthesis of 5,6'-dichloro-1-phenyl-3,3-dimethylspiroindoline benzopyran: In a round-bottom flask containing 30 parts of methanol solution, 3 parts of 5-chloro-1-phenyl-3,3-dimethyl-2-methyleneindoline and 1 part of 5-chlorosalicylaldehyde were added in sequence, a reflux condenser was installed, and the mixture was placed in a 70W ultrasonic cleaner and subjected to ultrasonic reflux reaction at 70°C in a water bath for 3 min. The mixture was filtered, dried, and cooled to obtain 5,6'-dichloro-1-phenyl-3,3-dimethylspiroindoline benzopyran.
[0077] Synthesis of 5,6'-diamino-1-phenyl-3,3-dimethylspiroindolinobenzopyran: Add 5 parts of 5,6'-dichloro-1-phenyl-3,3-dimethylspiroindolinobenzopyran into a round-bottom flask, add 25 parts of 10% ammonia methanol solution, place in a 70°C water bath, stir and reflux for 10 hours, distill off the excess solvent to obtain 5,6'-diamino-1-phenyl-3,3-dimethylspiroindolinobenzopyran.
[0078] H NMR spectrum: m / z: 369.18 (100.0%), 370.19 (26.3%), 371.19 (3.5%), 370.18 (1.1%), elemental analysis: C, 78.02; H, 6.27; N, 11.37; O, 4.33.
[0079] Synthesis of polyurea: Weigh 5 parts of 5,6'-diamino-1-phenyl-3,3-dimethylspiroindoline benzopyran and place them in a three-necked flask, stir and reflux in a 70°C water bath, prepare 1 part of solid phosgene and dissolve it in 50 parts of chloroform, slowly drop it into the above three-necked flask, and distill the excess solvent to obtain polyurea. Tested by ultraviolet spectrometer, the ultraviolet characteristic absorption peak of polyurea is 565nm, the absorption peak intensity is 0.10, when illuminated, the absorption peak intensity is 0.15, the increase is 50%, when stretched 350%, the absorption peak intensity is 0.10, the increase is 0%, and there is no color change. When the primary amine is excessive, the reaction generates a small molecule cyclic urea, and the color-changing group cannot be restored due to steric hindrance, which destroys the color-changing group.
[0080] Compared with Comparative Example 1 and Comparative Example 2, each polyurea segment of Examples 1-3 of the present invention contains a color-changing group, the color-changing group is evenly distributed, and the color changes sensitively under external stimuli. The color-changing group changes color repeatedly, and the number of reversible cycles determines the long-term color-changing performance of the material. In the reversible process of CO bond breaking, a photochemical side reaction occurs, resulting in color-changing failure. The scheme of the present application document has a high content of color-changing groups, which avoids the problem of color-changing failure of some color-changing groups.
[0081] Secondly, the polyurea polymer obtained by the four-step reaction has each molecular chain connected by a urea bond. The reaction does not involve polyols, and the corresponding product does not contain urethane bonds, but only urea bonds, which avoids the formation of bubbles when reacting with humid air. The polymer molecules are more stable and have better physical and mechanical properties. Moreover, the reaction does not require a catalyst, and there is no residual catalyst in the molecular chain. The material has good aging resistance and increases the service life of the material. The shortcomings of photochromic materials such as poor thermal stability and poor fatigue resistance are solved.
[0082] Thirdly, the color-changing polyurea provided by the present invention has readily available raw materials and low cost.
[0083] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A method for preparing a color-changing polyurea, characterized in that: The following steps are involved: Step 1. Synthesis of compound a Weigh NR-4-chlorophenylhydrazine, 3-methyl-2-butanone and triethylamine raw materials by weight, add them into a three-necked flask in sequence, heat in a water bath and stir to react under nitrogen protection, then add sodium carbonate to neutralize, collect the fractions by distillation to obtain product a; Step 2: Synthesis of Compound B In a round-bottom flask containing methanol solution, weighed compound a and 5-chlorosalicylaldehyde are added in sequence, a reflux condenser is installed, and the mixture is placed in an ultrasonic cleaner for water bath ultrasonic reflux reaction for 1-3 minutes, filtered, dried, and cooled to obtain compound b; Step 3. Synthesis of compound c Compound b was added to a round-bottom flask, and 10% ammonia methanol solution was added, and the mixture was placed in a water bath and stirred under reflux for 5-10 hours, and the excess solvent was distilled to obtain compound c; Step 4. Synthesis of Compound d Solid phosgene was dissolved in chloroform in a three-necked flask, and compound c was slowly added dropwise to the three-necked flask, and the mixture was stirred and refluxed in a water bath for reaction. After the addition was completed, the excess solvent was distilled off to obtain compound d, a color-changing polyurea. The expression of the preparation method of the color-changing polyurea is as follows: Among them, the R group is benzene and its derivatives.
2. The method for preparing the color-changing polyurea according to claim 1, characterized in that: In step 1, the three-necked flask is equipped with a stirrer, a thermometer and a reflux condenser device, and 2-6 parts of NR-based-4-chlorophenylhydrazine, 1-3 parts of 3-methyl-2-butanone and 1-3 parts of triethylamine are weighed by weight.
3. The method for preparing the color-changing polyurea according to claim 2, characterized in that: In step 1, under nitrogen protection, the reaction is heated in a water bath at 80° C. and stirred, then neutralized with 1-3 parts of sodium carbonate, and the fraction at 240-320° C. is collected by distillation to obtain product a.
4. The method for preparing the color-changing polyurea according to claim 3, characterized in that: The compound a is 1-5 parts of 5-chloro-1-R-3,3-dimethyl-2-methyleneindoline, wherein the R group of the compound a is benzene and its derivatives.
5. The method for preparing the color-changing polyurea according to claim 3, characterized in that: In step 2, 1-5 parts of compound a and 1-5 parts of 5-chlorosalicylaldehyde are added sequentially to a round-bottom flask containing 30 parts of methanol solution, a reflux condenser is installed, and the flask is placed in a 70W ultrasonic cleaner and ultrasonically refluxed at 70°C in a water bath for 1-3 minutes.
6. The method for preparing the color-changing polyurea according to claim 5, characterized in that: The purity of the 3-methyl-2-butanone and 5-chlorosalicylaldehyde is greater than or equal to 98%.
7. The method for preparing the color-changing polyurea according to claim 5, characterized in that: In step 3, 1-5 parts of compound b are added to a round-bottom flask, and 10-50 parts of 10% ammonia methanol solution are added, and the mixture is placed in a 70° C. water bath and stirred under reflux.
8. The method for preparing the color-changing polyurea according to claim 7, characterized in that: In step 4, 0.5-1 parts of solid phosgene is dissolved in 50 parts of chloroform in a three-necked flask, 4-6 parts of compound c are slowly added dropwise to the three-necked flask, and the mixture is stirred and refluxed in a 70° C. water bath for reaction.
9. The method for preparing the color-changing polyurea according to claim 8, characterized in that: The purity of the solid phosgene is ≥99.5%.
10. The method for preparing color-changing polyurea according to claim 7, characterized in that: The compound b is 5,6'-dichloro-1-benzyl-3,3-dimethylspiroindolinebenzopyran, and the compound c is 5,6'-diamino-1-benzyl-3,3-dimethylspiroindolinebenzopyran.
Citation Information
Patent Citations
Optical articles comprising photochromic poly(urea-urethane)
CN110537114A
Agent for coloring fibres, especially for temporary coloration of the hair, made by mixing prior to use of one component containing an enamine compound and another component containing at least one carbonyl compound
DE19933313A1
Thiadiazole derivatives
GB1400202A
Photochromic electrostatic toner compositions
US5759729A
Agent for coloring fibers
WO2000033799A1