A silane self-crosslinking cable insulation material and preparation method thereof, and new energy vehicle cable
Through the synergistic effect of component A and component B of the silane self-crosslinking cable insulating material, the problem of loosening of the aluminum alloy conductor and insulating material of new energy automobile cables is solved, and the high-temperature aging performance and safety are improved, meeting the requirements relevant standards.
Patent Information
- Application Number
- CN202211725648.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-30
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-12-30
AI Technical Summary
The aluminum alloy conductor of new energy vehicle cables is prone to loosening from the insulating material after irradiation, leading to potential safety hazards such as leakage and electric shock. Existing polyolefin materials that are resistant to long-term high temperature aging cannot completely solve this problem after irradiation.
The silane self-crosslinking cable insulation material is used. Through the synergy of specific A component and B component, the self-crosslinking reaction can occur without irradiation conditions, ensuring that the insertion and withdrawal force of the aluminum alloy conductor in the insulating material is greater than 100N. , prevent loosening, and meet the relevant performance requirements of ISO6722-1-2011 and JASO D618-2013.
It achieves the formation of stable insulating materials without irradiation conditions, prevents thermal expansion of aluminum alloy conductors, ensures safety and performance in compliance with standards, avoids leakage and electric shock hazards, and maintains softness and stable performance during long-term high temperature aging.
Smart Images

Figure CN115926304B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of automotive materials, and more specifically, to an insulating material for a silane self-crosslinking cable, a preparation method thereof, and a new energy vehicle cable. Background Art
[0002] New energy vehicles mainly include natural gas vehicles, hybrid vehicles and pure electric vehicles. Cables used in new energy vehicles need to meet the relevant performance requirements of ISO6722-1-2011 and JASO D618-2013.
[0003] Cable insulation materials for new energy vehicles are generally made of thermoplastic halogen-free flame-retardant elastomer TPE, or polyethylene (PE) and polyolefin elastomers, and have good softness after irradiation.
[0004] The core of cables for new energy vehicles is generally copper conductor, and the weight of the conductor accounts for more than 60% of the weight of the automotive cable. In order to achieve lightweight and low cost, new energy vehicles use aluminum alloy core as conductor, which can reduce the weight by more than 40% and reduce the cable cost by more than 30%.
[0005] Since the thermal expansion coefficient of aluminum conductors is significantly higher than that of copper conductors, when cable insulation materials are irradiated, the thermal expansion of aluminum alloy conductors is much greater than that of copper conductors, and the thermal expansion of aluminum alloy conductors will also stretch the insulation materials. After the aluminum alloy conductors cool and shrink after irradiation, looseness will occur between the aluminum alloy conductors and the stretched cable insulation materials, resulting in safety hazards such as leakage and electric shock.
[0006] The prior art discloses a polyolefin material resistant to long-term high temperature aging. After irradiation, the material has good softness, and the obtained new energy vehicle cable meets the relevant performance requirements of ISO6722-1-2011. However, since the insulating material for the new energy vehicle cable needs to be irradiated, when the cable uses aluminum alloy as the conductor, there will still be a problem of looseness between the aluminum alloy conductor and the insulating cable. Summary of the invention
[0007] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of the existing automotive aluminum alloy core cable insulation material that is easy to loosen with the aluminum alloy conductor after irradiation, and provide a silane self-crosslinking cable insulation material. Through the synergistic effect of specific A components and B components, a self-crosslinking reaction can occur without irradiation conditions. Since no electron beam irradiation is required, the aluminum alloy conductor in the insulation material will not undergo thermal expansion. The insertion and extraction force of the aluminum alloy conductor in the insulation material is greater than 100N, and there will be no looseness between the aluminum alloy conductor and the insulation material, thereby preventing safety hazards such as leakage and electric shock. The prepared automotive aluminum alloy core cable meets the relevant performance requirements of ISO6722-1-2011 and JASO D618-2013.
[0008] Another object of the present invention is to provide a method for preparing a silane self-crosslinking cable insulation material.
[0009] Another object of the present invention is to provide a new energy vehicle cable.
[0010] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0011] A silane self-crosslinking cable insulation material comprises a component A and a component B, wherein the weight ratio of the component A to the component B is (80-145): (25-40).
[0012] Wherein, component A includes, by weight, 30 to 60 parts of toughening agent; 40 to 60 parts of inorganic filler powder; 5 to 10 parts of bulking agent; 4 to 8 parts of antioxidant; 1 to 5 parts of organic tin catalyst; and 0 to 3 parts of processing aid.
[0013] Component B includes, by weight, 30 to 50 parts of polyethylene; 10 to 30 parts of toughening agent; 1 to 5 parts of silane coupling agent; and 1 to 5 parts of initiator.
[0014] The D50 of the inorganic filler powder is 1-7 um.
[0015] In the insulating material for new energy vehicle cables of the present invention, component A and component B can form silane self-crosslinking after mixing, and the content of component B is within the specific range of the present invention, and has a good degree of crosslinking. Since the self-crosslinking reaction can occur without irradiation conditions, since no electron beam irradiation is required, the aluminum alloy conductor in the insulating material will not undergo thermal expansion, the insertion and extraction force of the aluminum alloy conductor in the insulating material is greater than 100N, and there will be no looseness between the aluminum alloy conductor and the insulating material, preventing safety hazards such as leakage and electric shock.
[0016] The content of component B is relatively small, and the material will become brittle during the aging process with copper at 150°C for 3000 hours.
[0017] In the insulating material for new energy vehicle cables of the present invention, the amount of inorganic filler powder in component A is within the specific range of the present invention, so that the material has a smaller bending force and higher softness. If the amount of inorganic filler powder is too much, the surface of the finished cable will be pre-gelled during the extrusion process of components A and B, and the degree of crosslinking of different parts is uneven, which leads to extremely unstable thermal extension test and failure to pass the test, further resulting in the failure of a single vertical combustion test; and too much inorganic filler powder increases the content of metal impurity ions on the one hand, and the interface compatibility between too much inorganic filler powder and resin deteriorates on the other hand, resulting in poor long-term copper aging performance and elongation at break performance of the material.
[0018] Moreover, in order to further improve the softness of the material, in component A, polyethylene is 0 to 0.0000001 parts, that is, polyethylene is not included.
[0019] In component A, the amount of antioxidant used is higher than that of general cable formulas. Even if a higher amount of antioxidant is used, it is difficult to precipitate on the cable surface. Antioxidants are beneficial to improving the material's resistance to long-term thermal oxidative aging.
[0020] In component A, the organotin catalyst can increase the cross-linking efficiency of component A and component B, and the thermal elongation is low, which is beneficial to improve the copper aging performance of the material. However, if the amount of organotin catalyst is too large, the elongation at break of the material will be significantly reduced.
[0021] The D50 of the inorganic filler powder is greater than 7μm. If the powder particle size is too large, the elongation at break of the material will be significantly reduced. If the D50 of the inorganic filler powder is too small, the powder fluidity is very poor, the extrusion speed is slow when components A and B are self-crosslinked, and forcibly increasing the screw speed will damage the equipment.
[0022] Preferably, in component A, the inorganic filler powder is 45 to 55 parts.
[0023] Preferably, the inorganic filler powder is one or more of magnesium hydroxide, aluminum hydroxide, calcium carbonate, high clay, white carbon black, hypophosphite or melamine cyanurate, and the activation degree of the inorganic filler powder is less than or equal to 10%, and the test standard of the activation degree is GB / T 19281-2014.
[0024] The activation degree of the inorganic filler powder is less than or equal to 10%, which can prevent the moisture in the powder from causing the A component to be pre-crosslinked in advance, thereby preventing the copper aging performance of the material from being reduced.
[0025] The inorganic filler powder has a small particle size, which is beneficial to improving the flame retardancy and elongation at break of the material.
[0026] Preferably, the organotin catalyst is one or more of dibutyltin dilaurate, dioctyltin dilaurate or di(dodecylthio)dibutyltin.
[0027] Preferably, the silane coupling agent is vinyltrimethoxysilane, vinyltriethoxysilane or vinyltri(2-methoxyethoxy)silane, and the initiator is one or more of di-tert-butyl peroxide, 2,3-dimethyl-2,3-diphenylbutane or 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane.
[0028] Preferably, in the components A and B, the toughening agent is one or more of POE, EVA, EEA, TPE, TPU, EMA, EBA, and EPDM, and the density of the toughening agent is 0.85 to 1.2 g / cm 3 The melt index under the test conditions of 230℃ and 2.16Kg is 0.5~20g / 10min, and the test standard is GB / T3682-2000.
[0029] Preferably, the compatibilizer is one or more of POE-g-MAH, LLDPE-g-MAH, EVA-g-MAH or EXA-g-MAH.
[0030] The melt index of the compatibilizer under the test conditions of 190°C and 2.16kg is 1-8g / 10min.
[0031] Preferably, the polyethylene is LDPE and / or LLDPE, with a density of 0.87-0.92 g / cm 3 The melt index under the test conditions of 190℃ and 2.16Kg is 0.1~5g / 10min, and the test standard is GB / T3682-2000.
[0032] Preferably, the antioxidant is one or more of a hindered amine antioxidant, a hindered phenol antioxidant, a phosphite antioxidant or a hydrazide antioxidant.
[0033] Among them, the hindered amine antioxidant can be 445 and / or 944, the hindered phenol antioxidant can be one or more of 1010, 1076, 1079 or 1035, the phosphite antioxidant can be one or more of 168, RIANOX DSTDP or PEP-36, and the hydrazide antioxidant can be SONOX 1027 and / or RIANOX MD-1024.
[0034] Antioxidants can enhance the antioxidant effect of silane self-crosslinking cable insulation materials.
[0035] In practical applications, the processing aid is a lubricant, which can be at least one of a fluorine lubricant, a polyethylene wax lubricant, a silicone masterbatch lubricant or a stearic acid lubricant.
[0036] More preferably, the lubricant is a silicone masterbatch lubricant.
[0037] Lubricants can improve the lubrication effect of silane self-crosslinking cable insulation materials.
[0038] The present invention also protects a method for preparing the above-mentioned silane self-crosslinking cable insulating material, comprising the following steps:
[0039] S1. The A component is mixed evenly, and kneaded and plasticized by a reciprocating machine at 100 to 200°C to obtain material A;
[0040] The B component is mixed evenly, extruded and granulated at 90-200°C by a twin-screw extruder, and dried to obtain material B.
[0041] S2. Extrusion molding material A and material B at 90-180° C. to obtain silane self-crosslinking cable insulation material.
[0042] The present invention also protects a new energy vehicle cable, comprising an aluminum alloy conductor and an insulating material wrapping the aluminum alloy conductor, wherein the insulating material is the insulating material for the silane self-crosslinking cable described above.
[0043] The finished cable for new energy vehicles of the present invention has good softness, does not cause brittle cracking after long-term high-temperature aging with copper at 150° C. for 3000 h, meets the relevant performance requirements of ISO6722-1-2011 and JASO D618-2013, and is particularly suitable for new energy vehicle cables with aluminum alloy conductors as wire cores.
[0044] Compared with the prior art, the present invention has the following beneficial effects:
[0045] The invention discloses an insulating material for a silane self-crosslinking cable. The insulating material can be self-crosslinked without irradiation conditions through the synergistic effect of a specific A component and a B component. Since no irradiation is required, the aluminum alloy conductor in the insulating material will not undergo thermal expansion. The insertion and extraction force of the aluminum alloy conductor in the insulating material is greater than 100N. The aluminum alloy conductor and the insulating material will not be loose, thereby preventing safety hazards such as leakage and electric shock. The prepared automotive aluminum alloy core cable meets the relevant performance requirements of ISO6722-1-2011 and JASO D618-2013.
[0046] The silane self-crosslinking cable insulation material of the present invention has a smooth surface after extrusion, only slight pre-crosslinking occurs, and further can achieve no gel point. The Shore hardness is 81-90 and can be used to prepare 10-120mm2 The wire can pass the horizontal flame retardant test. The finished cable does not become brittle after copper aging at 150℃ / 3000h. The tensile strength of the finished cable can reach 11-13MPa, and the elongation at break can reach 300-415%. At 200℃ and 0.2MPa, the thermal extension of the finished cable can reach 40-50%, and the insertion and extraction force of the aluminum alloy conductor in the insulating material can reach 116-122N. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 This is an appearance picture of the cable in Example 2 with no gel spots on the surface.
[0048] Figure 2 This is an appearance picture of the pre-gel produced on the cable surface of Comparative Example 1. DETAILED DESCRIPTION
[0049] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.
[0050] Component A:
[0051] The toughening agent is ethylene-vinyl acetate copolymer EVA: 7350M, with a melt index of 4g / 10min and a density of 0.936g / cm under the test conditions of 190℃ and 2.16kg. 3 , Yangzi Petrochemical;
[0052] Inorganic filler powder 1 is aluminum hydroxide: ATH-1, D50 is 3um, activation degree is 5%, China Aluminum Corporation and American MARTINAL;
[0053] Inorganic filler powder 2 is magnesium hydroxide: MDH-2500g, D50 is 2.5μm, activation degree is 5%, Yingkou, Liaoning;
[0054] Inorganic filler powder 3 is magnesium hypophosphite: brand M16S, D50 is 3 μm, activation degree is 5%, and the manufacturer is Kingfa Technology Co., Ltd.;
[0055] Inorganic filler powder 4 is magnesium hydroxide: JS-MDH03, D50 is 3 μm, activation degree is 90%, Jiangsu Magnesium Aluminum Chemical Industry;
[0056] Inorganic filler powder 5 is aluminum hydroxide: ALH-03, D50 is 18 μm, activation degree is 0%, and the manufacturer is Shandong Weihai Chemical;
[0057] The compatibilizer is EVA grafted maleic anhydride EVA-g-MAH: C150, with a melt index of 1.5 g / 10 min at 190 °C and 2.16 kg, from Kingfa Science & Technology Co., Ltd.
[0058] The antioxidants are hindered phenol antioxidants, phosphite antioxidants and hydrazide antioxidants, the mass ratio of hindered phenol antioxidants, phosphite antioxidants and hydrazide antioxidants is 1:5:1, they are commercially available and the same one is used in parallel experiments;
[0059] The organotin catalyst was di(dodecylthio)dibutyltin, which is commercially available and the same one was used in parallel experiments;
[0060] The processing aid was a silicone masterbatch lubricant, which was commercially available and the same one was used in parallel experiments;
[0061] Component B:
[0062] Polyethylene is linear low-density polyethylene LLDPE, LLDPE 7040, with a density of 0.915 g / cm 3 , the melt index under the test conditions of 190℃ and 2.16kg is 2g / 10min, Sinopec;
[0063] The toughening agent is ethylene-vinyl acetate copolymer EVA: EVA 7350M, with a melt index of 4 g / 10 min and a density of 0.936 g / cm under the test conditions of 190°C and 2.16 kg. 3 , Yangzi Petrochemical;
[0064] The silane coupling agent is vinyl trimethoxysilane, G-172, Sibao Technology;
[0065] The initiator was 2,3-dimethyl-2,3-diphenylbutane, which is commercially available and the same one was used in parallel experiments.
[0066] Examples 1 to 14
[0067] A silane self-crosslinking cable insulation material, comprising component A and component B, by weight, wherein component A comprises, by weight, a toughening agent; an inorganic filler powder; a compatibilizer; an antioxidant; an organic tin catalyst; and a processing aid;
[0068] Component B includes polyethylene, a toughening agent, a silane coupling agent, and an initiator in parts by weight.
[0069] Component B is divided into 30 parts.
[0070] The specific content of each component is shown in Table 1 below.
[0071] Table 1 Composition of silane self-crosslinking cable insulation materials in various embodiments (by weight)
[0072]
[0073]
[0074] Table 1
[0075]
[0076]
[0077] Table 1
[0078]
[0079] The preparation method of the above-mentioned silane self-crosslinking cable insulation material is as follows:
[0080] S1. The A component is mixed evenly, and kneaded and plasticized by a reciprocating machine at 100 to 200°C to obtain material A;
[0081] The B component is mixed evenly, extruded and granulated at 90-200°C by a twin-screw extruder, and dried to obtain material B.
[0082] S2. Extrusion molding material A and material B at 90 to 180°C to obtain a silane self-crosslinking cable insulation material;
[0083] Among them, component A is mixed and evenly dispersed through the reciprocating soft shearing between the threads of the reciprocating machine, the melt of component A and the pins; the main machine screw speed is 50-300r / min, and the feed rate is 100-500Kg / h.
[0084] Comparative Examples 1 to 9
[0085] An insulating material, comprising component A and component B, by weight, wherein component A comprises, by weight, a toughening agent; an inorganic filler powder; a compatibilizer; an antioxidant; an organic tin catalyst; and a processing aid;
[0086] Component B includes polyethylene, a toughening agent, a silane coupling agent, and an initiator in parts by weight.
[0087] Component B is divided into 30 parts.
[0088] The specific content of each component is shown in Table 2 below.
[0089] Table 2 Composition of silane self-crosslinking cable insulation materials of each comparative example (by weight)
[0090]
[0091]
[0092] Table 2
[0093]
[0094]
[0095] The preparation method of the above silane self-crosslinking cable insulation material is the same as that of Examples 1 to 9, which will not be described in detail here.
[0096] Comparative Example 10
[0097] An insulating material, wherein the contents of each component are the same as those in Example 1.
[0098] The difference from Example 1 is the preparation method:
[0099] S1. The A component is mixed evenly, and mixed and plasticized and granulated at 100 to 200° C. by a twin-screw extruder to obtain material A;
[0100] The B component is mixed evenly, extruded and granulated at 90-200°C by a twin-screw extruder, and dried to obtain material B.
[0101] S2. Extrusion molding material A and material B at 90-180°C to obtain insulating material.
[0102] Comparative Example 11
[0103] An insulating material comprises, by weight, 3 parts of low-density polyethylene, 40 parts of EVA, 50 parts of aluminum hydroxide 1, 10 parts of EVA-g-MAH, 1 part of trimethylolpropane triacrylate and 1 part of antioxidant.
[0104] The preparation method is as follows:
[0105] S1. Select a continuous multi-field coupling strong shearing method to plasticize and granulate all components except the inorganic filler powder; wherein the continuous multi-field coupling strong shearing method is a twin-screw extrusion method using a strong shear meshing thread element combined with a tensile thread element and then combined with a strong shear meshing thread element; the process conditions are a temperature of 200°C, a feeding capacity of 450kg / h, and a screw speed of 400rpm;
[0106] S2. Select the intermittent multi-field coupling weak shear method, plasticize and granulate the granulated material obtained in S1 with the inorganic filler powder to obtain a high flame retardant grade, low smoke and halogen-free material; wherein, the intermittent multi-field coupling weak shear method is to first adopt internal mixing and then adopt a single screw extrusion method with a screw compression ratio of 1 to 2; the process conditions are internal mixing rotor 80r / min, internal mixing temperature 150℃; single screw speed 150rpm, temperature 200℃.
[0107] S3. Radiation cross-linking: irradiation dose 20 Mrad.
[0108] Results
[0109] The silane self-crosslinking cable insulation materials of the above embodiments and comparative examples were tested for relevant properties, including hardness and flame retardancy. The specific testing methods are as follows:
[0110] Hardness: The implementation standard is GB / T 2411-2008, and the unit is Shore hardness A;
[0111] Flame retardant properties include: V-1 grade UL94 vertical burning test (thickness 3.0mm) and ISO6722-1-2011 horizontal flame retardant burning test;
[0112] The silane self-crosslinking cable insulation materials of the above embodiments and comparative examples were prepared into finished cables for new energy vehicles, and the cables for new energy vehicles were subjected to relevant performance tests, including: long-term high-temperature copper aging performance, tensile strength, elongation at break, thermal elongation, and plug-in force performance tests. The specific testing methods are as follows:
[0113] Long-term high-temperature copper aging performance: finished cable 150℃ / 3000h copper aging, implementation standard ISO6722-1-2011;
[0114] Tensile strength: tested according to GB / T 1040.3-2006 standard;
[0115] Elongation at break: Tested according to GB / T 1040.3-2006 standard;
[0116] Thermal elongation: Tested at 200℃ and 0.2MPa according to GB / T2951.21-2008 standard, if the thermal elongation of the finished cable is too large or even breaks, it means that the cross-linking is not sufficient or has not occurred;
[0117] Insertion and extraction force test, the test method is: GB / T 2792-2014;
[0118] The specific test results of each embodiment are described in Table 3 below:
[0119] Table 3
[0120]
[0121]
[0122] Table 3
[0123]
[0124] Table 3
[0125]
[0126]
[0127] The specific test results of each comparative example are described in Table 4 below:
[0128] Table 4
[0129]
[0130]
[0131] Table 4
[0132]
[0133] It can be seen from the above results that the insulating material prepared by the newly developed reciprocating machine production process under the component dosage ratio required by the present invention has uniform particle size and a uniform surface without powder spots; it is suitable for production line gauge of 2.5mm 2 ~120mm 2 The new energy vehicle cables have good softness after irradiation, and will not become brittle or crack after long-term high-temperature aging with copper at 150°C for 3000h. The new energy vehicle cables fully meet the relevant performance requirements of ISO6722-1-2011 and JASO D618-2013.
[0134] It can be seen from Examples 1 and 2 that a smaller amount of toughening agent is used in component A, which will reduce the elongation at break.
[0135] It can be seen from Examples 2 to 5 that hypophosphite is softer than magnesium hydroxide and aluminum hydroxide, and therefore, Example 5 has the lowest hardness.
[0136] It can be seen from Example 2, Example 6 and Example 7 that the use amount of inorganic filler powder is small, which is beneficial to improve the elongation at break, reduce the hardness and improve the softness.
[0137] It can be seen from Example 2 and Example 8 that the inorganic filler powder is activated inorganic filler powder, and component A is prone to cross-linking in advance, resulting in poor copper aging performance of the insulating material.
[0138] The materials of Example 9 and Example 10 are softer in hardness and have slightly smaller insertion and extraction forces.
[0139] It can be seen from Example 2 and Comparative Example 1 that the amount of inorganic filler powder used is too much. After A / B compounding, the elongation at break of the material is significantly reduced. At the same time, too much powder can easily cause excessive frictional heat generation during processing, resulting in premature generation of pre-gel.
[0140] It can be seen from Example 2 and Comparative Example 2 that the amount of inorganic filler powder used is too small, resulting in a lower content of material B relative to the entire resin, which leads to lower crosslinking efficiency, or even failure to crosslink, and the copper aging performance will also be unqualified.
[0141] It can be seen from Example 2 and Comparative Example 3 that without adding an organic tin catalyst, the cross-linking efficiency becomes low, or even cross-linking fails, and the copper aging performance is also unqualified.
[0142] It can be seen from Example 2 and Comparative Example 4 that excessive use of the organotin catalyst will result in premature pre-gelation, poor extrusion appearance, and significantly reduced elongation at break.
[0143] It can be seen from Example 2 and Comparative Example 5 that without adding an initiator, the cross-linking efficiency becomes low, and even cross-linking cannot be achieved, and the copper aging performance of the strip will also be unqualified.
[0144] It can be seen from Example 2 and Comparative Example 6 that the amount of initiator used is too large, the crosslinking is too fast, pre-gel occurs, the extrusion appearance is not good, and the elongation at break is also significantly reduced.
[0145] It can be seen from Example 2 and Comparative Example 7 that if the D50 of the inorganic filler powder is too large, the elongation at break of the material will be significantly reduced.
[0146] It can be seen from Example 2 and Comparative Example 8 that the content of component B is too little, and the weight ratio of component A to component B is too large. When A and B are mixed and extruded, the finished product cannot be effectively cross-linked, because the less component B is, the fewer cross-linking points there are.
[0147] It can be seen from Example 2 and Comparative Example 9 that the content of component A is too little, and the weight ratio of component A to component B is too small. When A and B are mixed and extruded, the finished product is very likely to have pre-gel, which is equivalent to having too many cross-linking points that play a cross-linking role.
[0148] It can be seen from Example 2 and Comparative Example 10 that component A adopts a twin-screw extruder, which has a continuous strong shear screw, foaming occurs during the production process, pre-gel appears on the surface of the finished cable, and the elongation at break of the finished cable cannot meet the requirements of ISO6722-1-2011.
[0149] It can be seen from Example 2 and Comparative Example 11 that although the cable of Comparative Example 8 meets the relevant performance requirements of ISO6722-1-2011 and JASOD618-2013, the cable preparation process requires electron beam irradiation, the aluminum alloy conductor in the insulating material undergoes thermal expansion, the insertion and extraction force of the aluminum alloy conductor in the insulating material is 80N, and the aluminum alloy conductor and the insulating material are prone to looseness, which is prone to safety hazards such as leakage and electric shock.
[0150] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A silane self-crosslinking cable insulation material, It is characterized in that The composition comprises component A and component B, wherein the weight ratio of component A to component B is (80-119): (30-40). Wherein, component A includes, by weight, 30 to 60 parts of toughening agent; 40 to 60 parts of inorganic filler powder; 5 to 10 parts of bulking agent; 4 to 8 parts of antioxidant; 1 to 5 parts of organic tin catalyst; and 0 to 3 parts of processing aid. Component B includes, by weight, 30 to 50 parts of polyethylene; 10 to 30 parts of toughening agent; 1 to 5 parts of silane coupling agent; and 1 to 5 parts of initiator. The D50 of the inorganic filler powder is 1 to 7 um; The activation degree of the inorganic filler powder is less than or equal to 10%, and the test standard of the activation degree is GB / T19281-2014; The initiator is one or more of di-tert-butyl peroxide, 2,3-dimethyl-2,3-diphenylbutane or 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane.
2. The silane self-crosslinking cable insulation material according to claim 1, It is characterized in that In component A, the inorganic filler powder is 45 to 55 parts.
3. The silane self-crosslinking cable insulation material according to claim 1, It is characterized in that The inorganic filler powder is one or more of magnesium hydroxide, aluminum hydroxide, calcium carbonate, white carbon black or hypophosphite.
4. The silane self-crosslinking cable insulation material according to claim 1, It is characterized in that The organic tin catalyst is one or more of dibutyltin dilaurate, dioctyltin dilaurate or di(dodecylthio)dibutyltin.
5. The silane self-crosslinking cable insulation material according to claim 1, It is characterized in that The silane coupling agent is one or more of vinyl trimethoxy silane, vinyl triethoxy silane or vinyl tri (2-methoxyethoxy) silane.
6. The silane self-crosslinking cable insulation material according to claim 1, It is characterized in that In the components A and B, the toughening agent is one or more of POE, EVA, EEA, TPE, TPU, EMA, EBA, and EPDM, and the density of the toughening agent is 0.85 to 1.2 g / cm 3 The melt index under the test conditions of 230℃ and 2.16Kg is 0.5~20g / 10min, and the test standard is GB / T 3682-2000.
7. The silane self-crosslinking cable insulation material according to claim 1, It is characterized in that The compatibilizer is one or more of POE-g-MAH, LLDPE-g-MAH or EVA-g-MAH.
8. The silane self-crosslinking cable insulation material according to claim 1, It is characterized in that The polyethylene is LDPE and / or LLDPE, and has a density of 0.87-0.92 g / cm 3 The melt index under the test conditions of 190℃ and 2.16Kg is 0.1~5g / 10min, and the test standard is GB / T 3682-2000.
9. A method for preparing the silane self-crosslinking cable insulation material according to any one of claims 1 to 8, It is characterized in that The steps include: S1. The A component is mixed evenly, and kneaded and plasticized by a reciprocating machine at 100 to 200°C to obtain material A; Mix component B evenly, extrude and granulate at 90-200°C through a twin-screw extruder, and obtain material B after drying; S2. Extrusion molding material A and material B at 90-180° C. to obtain silane self-crosslinking cable insulation material.
10. A new energy vehicle cable, It is characterized in that The invention comprises an aluminum alloy conductor and an insulating material wrapping the aluminum alloy conductor, wherein the insulating material is the insulating material for a silane self-crosslinking cable according to any one of claims 1 to 8.
Citation Information
Patent Citations
Self-crosslinking polyolefin material as well as preparation method and application thereof
CN114685880A