Positive electrode active material, lithium ion secondary battery and electrical equipment
By controlling the particle size and conductivity of lithium nickel cobalt manganese oxide or lithium nickel cobalt aluminum oxide, the problem of degradation of kinetics and rate performance of ternary positive electrode materials when the cobalt content decreases, achieving high capacity, magnification and cycle The improvement in performance extends the life of lithium-ion secondary batteries.
Patent Information
- Application Number
- CN202211447639.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-18
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-11-18
AI Technical Summary
When the cobalt content of the existing ternary positive electrode materials decreases, the lithium ion deintercalation kinetics will deteriorate, resulting in a significant decrease in battery capacity and initial power, a decrease in rate performance, poor surface structure stability, serious growth in cyclic impedance, affecting the long-term life of the battery.
By controlling the particle size, conductivity and compaction density of lithium nickel cobalt manganese oxide or lithium nickel cobalt aluminum oxide, it is ensured that it meets specific relationships (0.42≤U≤4.50), to improve kinetic performance and cycling performance and reduce the Impedance during fast charging extends battery life.
It realizes that under low cobalt content, lithium-ion secondary batteries have high capacity, rate performance and cycle performance, improve fast charging cycle life, and reduce performance attenuation and safety hazards caused by excessive impedance.
Smart Images

Figure CN115939337B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of secondary batteries, and in particular to a positive electrode active material, a lithium ion secondary battery and an electrical device. Background Art
[0002] The positive electrode material is one of the most critical materials affecting the performance of lithium-ion batteries. Ternary materials have been widely used in the field of power batteries due to their high energy density. However, due to the low reserves and high cost of cobalt resources, the price of ternary materials is much higher than that of lithium iron phosphate. Therefore, reducing the cobalt content in ternary materials has become one of the effective means to reduce battery costs. However, when the cobalt content of existing ternary materials decreases, the lithium ion insertion and extraction kinetics deteriorate, which will cause a significant decrease in the capacity and initial power of the battery; at the same time, it will also affect the rate performance of the material, making it difficult to adapt to the existing high-rate fast charging; moreover, when the cobalt content is low, the surface structural stability of the material will also deteriorate, and the surface side reactions will increase, resulting in a rapid decay of its long-term life and a serious deterioration of the cycle impedance growth. Therefore, it is necessary to provide a low-cobalt ternary positive active material that takes into account capacity, rate performance and cycle performance. Summary of the invention
[0003] The present application aims to solve at least one of the technical problems existing in the prior art. To this end, the present application proposes a low-cobalt ternary positive electrode active material, which can take into account good capacity, cycle performance and rate performance.
[0004] In a first aspect of the present application, a positive electrode active material is provided, the positive electrode active material comprising at least one of lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide, and the positive electrode active material satisfies 0.42≤U≤4.50;
[0005] Where U=6K / (π·D v 99 2 C),
[0006] K is the conductivity of the positive electrode active material under a pressure of 60 MPa, in μs / cm;
[0007] D v 99 is the particle size corresponding to when the cumulative volume distribution percentage of the positive electrode active material reaches 99%, in μm;
[0008] C is the compaction density of the positive electrode active material at 60 MPa, in g / cm 3 .
[0009] The positive electrode active material according to the embodiment of the present application has at least the following beneficial effects:
[0010] In the present application, by controlling the particle size of the positive electrode active material, the resistivity of the positive electrode active material and the positive electrode active compaction density, and making the three satisfy the above-mentioned relationship at the same time, the low-cobalt material has a higher capacity, and at the same time can meet the low impedance requirements during fast charging, and can effectively reduce heat generation at high rates, thereby improving safety performance; and under the premise of ensuring kinetic performance, it can slow down the accelerated capacity decay and increase the fast charging cycle life.
[0011] For the positive electrode active materials in this application, lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide include secondary particles formed by agglomeration of primary particles. It is understood that the presence of separate primary particles is not excluded in the positive electrode active materials, such as primary particles that have not been aggregated into secondary particles, or primary particles that are re-peeled off from secondary particles in a crushing process, etc. Therefore, D v 99 refers to the particle size corresponding to the cumulative volume distribution percentage of all positive electrode active materials including primary particles and secondary particles reaching 99%. Similarly, if it exists, D v 50 refers to the particle size corresponding to the cumulative distribution percentage of the volume of all positive electrode active materials including primary particles and secondary particles reaching 50%, D v 10 refers to the particle size corresponding to the cumulative distribution percentage of the volume of all positive electrode active materials including primary particles and secondary particles reaching 10%. v 99.D v 50. D v 10 and the correlation therebetween can reflect the particle size and distribution of the positive electrode active material, and the specific values thereof can be obtained by relevant methods and / or instruments known in the art, for example, the above parameters can be measured by a laser particle size analyzer.
[0012] In the positive electrode active material, it contains multiple particles of lithium nickel cobalt manganese oxide and / or lithium nickel cobalt aluminum oxide, which is a powder collection composed of primary particles and secondary particles. Therefore, the conductivity of the positive electrode active material refers to the conductivity of this powder as a whole. Therefore, it should be noted that the conductivity K of the positive electrode active material is affected by the conductivity of the lithium nickel cobalt manganese oxide particles, the particle size distribution of the lithium nickel cobalt manganese (and / or aluminum) oxide particles in the positive electrode active material, and the tightness of the accumulation of lithium nickel cobalt manganese (and / or aluminum) oxide particles in the positive electrode active material. The overall conductivity of the positive electrode active material is reflected. The specific value of the conductivity K of the positive electrode active material can be obtained by related methods and / or instruments known in the art, for example, its conductivity can be calculated by measuring the resistivity, including measuring the conductivity of the positive electrode active material using a four-probe method. Specifically, the positive electrode active material can be placed in a container and pressure is applied, and the voltage drop on the positive electrode active material is measured after the current is passed to obtain the resistivity and conductivity. Therefore, its conductivity also has a certain relationship with the pressure applied thereto. In this application, a pressure of 60MPa is used as a measurement standard. In some specific embodiments, the test method of conductivity is: using the four-probe method, the positive electrode active material is placed in a container and pressurized to a pressure of 60MPa, and the resistivity is obtained by reading 5s after stabilization, and the reciprocal is taken to obtain the conductivity. Similarly, the compaction density C of the positive electrode active material is related to factors such as the particle size and particle size distribution of the lithium nickel cobalt manganese (and / or aluminum) oxide particles therein, reflecting the compaction ability of the positive electrode active material. The test method of compaction density C is: a certain mass of positive electrode active material is placed in a mold, pressurized to 60MPa, and the height value is recorded 5s after stabilization. The compaction density is calculated by the sample mass, height and mold area. The compaction density of the positive electrode active material in the positive electrode active material layer can be collected by calcining the positive electrode active material and then tested.
[0013] From the above, it can be seen that in the scheme of the present application, the positive electrode active material is controlled to satisfy the above relationship, the unit mass conductivity of the particles in the positive electrode active material is guaranteed, the primary particles, the secondary particles, and the primary and secondary particles in the positive electrode active material are in closer contact, the transmission path of lithium ions between particles is shortened, the kinetic performance of the positive electrode active material is improved, and the kinetic problems caused by the decrease in cobalt content in low-cobalt materials are further improved, and the positive electrode active material is guaranteed to have a high lithium ion and electron transmission capacity, so that the lithium ion secondary battery prepared using this positive electrode active material still has a high cycle life under high rate conditions; at the same time, the positive electrode plate using the positive electrode active material has a high conductivity, which can ultimately ensure that the lithium ion secondary battery meets the extremely high impedance requirements of fast charging technology, improve power performance, and at the same time greatly reduce the performance degradation and safety hazards caused by heat generation due to excessive impedance to the battery.
[0014] In some embodiments of the present application, low cobalt means that the total molar amount of metal elements other than lithium in the positive electrode active material is 100%, and the molar percentage of cobalt element does not exceed 25%, for example, no more than 25%, 24%, 23%, 22%, 21%, 20%, 19%, 18%, 17%, 16%, 15%, 14%, 13%, 12%, 11%, 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1%. Since cobalt in the positive electrode material is mainly used to improve its conductivity and enhance the rate performance of the material, in order to improve its fast charging capability, in some specific embodiments, the molar percentage of cobalt element is not less than 0.01%, for example, not less than 0.01%, 0.02%, 0.05%, 0.1%, 0.2%, 0.5%, 1%, 2%, 3%, 4%, 5%. Furthermore, based on the total molar amount of metal elements other than lithium in lithium nickel cobalt manganese oxide or lithium nickel cobalt aluminum oxide as 100%, the molar percentage of cobalt element is 0.1-25%, 1-20%, 5-15%. It can be understood that in some of these methods, low cobalt does not exclude the situation where the cobalt content is extremely low and can be regarded as zero cobalt-free.
[0015] In some embodiments of the present application, U is 1.00 to 4.00. Further, U is 1.30 to 3.50.
[0016] In some embodiments of the present application, the positive electrode active material satisfies at least one of the following (i) to (iii):
[0017] (i)180μs / cm≤K≤430μs / cm;
[0018] (ii) 8 μm ≤ D v 99≤14μm;
[0019] (iii) 3.1 g / cm 3 ≤C≤3.7g / cm 3 .
[0020] When the particle size D v When the particle size is too small, although the transmission path of lithium ions becomes shorter and the kinetic performance is improved, the specific surface area of particles that are too small will increase, which will intensify the side reaction between the particles of the positive electrode active material and the electrolyte, accelerate the decay of the capacity retention rate under high rate conditions, and reduce the fast charging performance. v When 99 is too large, the dynamic performance deteriorates, the capacity decreases, the impedance increases, the heat generation increases under high rate conditions, and the temperature rise during fast charging is more obvious. On the other hand, the physical properties of the particles are interrelated, D v99 increases, which will, to a certain extent, reduce the conductivity K value, thereby reducing the U value. Similarly, the compaction density C is related to the particle size of the lithium nickel cobalt manganese particles and their particle size distribution. Too large or too small a compaction density will also cause a decrease in the kinetic performance and / or fast charging performance of the positive electrode active material, while within a certain range, the lithium-ion secondary battery can have a higher energy density and power performance. Therefore, in some specific embodiments, K is limited to between 180 and 430 μs / cm; and / or, D v 99 is between 8 and 14 μm; and / or C is between 3.1 and 3.7 g / cm 3 between.
[0021] In some embodiments of the present application, the positive electrode active material satisfies 2.5 μm ≤ D v 50≤6μm, D v 50 is the particle size corresponding to the cumulative volume distribution percentage of the particles reaching 50%. Furthermore, the positive electrode active material satisfies 2.5μm≤D v 50≤5μm.
[0022] In some embodiments of the present application, the positive electrode active material satisfies 2.5 μm ≤ D v 50≤6μm, 8μm≤D v 99≤14μm.
[0023] In some embodiments of the present application, the positive electrode active material satisfies 2.5 μm ≤ D v 50≤5μm, 8μm≤D v 99≤14μm.
[0024] At the same time, D v 50 and D v 99 requires that there will not be too many small particles in the positive electrode active material, which can effectively reduce the side reaction between the particle surface interface and the electrolyte caused by the increase in specific surface area due to the decrease in particle size, reduce battery gas expansion, and improve the high temperature performance and safety performance of the positive electrode active material. In addition, the particle size of the positive electrode active material satisfies the above-mentioned predetermined relationship, which can ensure that the positive electrode active material can reduce the decrease in the material kinetic capacity caused by the increase in the transmission path of lithium ions between particles due to the excessive size of the particles, and can effectively improve the rate performance and power performance of the battery. Moreover, this uniform combination of large and small particles can further improve the compaction density of the positive electrode active material, so that the positive electrode sheet has a more uniform surface density and a higher compaction density, and ultimately greatly improves the capacity, cycle performance and energy density of the lithium-ion secondary battery.
[0025] In some embodiments of the present application, lithium nickel cobalt manganese oxide and / or lithium nickel cobalt aluminum oxide comprises a general formula of Li x Nia Co b R c Me d O e Z f Compounds, wherein 0.8≤x≤1.2, a+b+c+d=1, b≤0.25, d≤0.12, e≥1, e+f≤2, and a-f are not negative numbers;
[0026] Me includes at least one of Al, Zr, Sr, Ti, B, Mg, Sn, W, Y, Ba, Nb, Mo, Ta, Si, La, Er, Nd, Gd, and Ce;
[0027] Z includes at least one of P, S, N, F, Cl, Br, and I;
[0028] R includes at least one of Mn and Al.
[0029] Wherein, when d=f=0, lithium nickel cobalt manganese oxide and / or lithium nickel cobalt aluminum oxide is a lithium ternary positive electrode material that has not been doped or coated. In order to reduce the degradation of rate performance and cycle performance caused by lithium precipitation caused by the mixing of nickel and lithium, lithium nickel cobalt manganese oxide and / or lithium nickel cobalt aluminum oxide may also be doped with other metal elements or non-metal elements. These metal or non-metal elements may be modified in the form of at least one of oxides, hydroxides, salts, etc. to achieve doping.
[0030] If d is not 0, the electrochemical properties of nickel cobalt manganese oxide and / or lithium nickel cobalt aluminum oxide, such as various properties of lithium ion secondary batteries, can be further improved by doping with the Me element.
[0031] In some embodiments of the present application, Me includes at least one of Al, W, and Zr. Al doping can stabilize the main structure of the particles and improve the long cycle performance; W doping can refine the particles, form lithium tungstate fast ion conductors on the surface of the particles, and improve the kinetic properties of the material; Zr doping forms a strong chemical bond with oxygen in the material, plays a supporting role in the transition metal layer, and improves the long cycle life and kinetic properties of the material.
[0032] In some embodiments of the present application, 0.55≤a≤0.7, 0.05≤b≤0.25, and 0.09≤c≤0.3.
[0033] In the above embodiment, by controlling the cobalt content in the positive electrode active material at a relatively low level, the use of rare metal cobalt is reduced, and the cost can be effectively reduced. At the same time, each element in the positive electrode active material satisfies the predetermined relationship in the general formula, which can ensure that the transition metal layer and the lithium layer in the ternary layered oxide are arranged in an orderly manner, and maintain a good layered structure, which is conducive to the high kinetic performance of lithium ions and electrons in the positive electrode active material particles, and can ensure that the lithium ion secondary battery has a high capacity, power performance, rate performance and long-term cycle performance. In addition, a higher nickel content is also beneficial to the capacity and energy density of the battery.
[0034] In some embodiments of the present application, 0.2
[0035] In some embodiments of the present application, d≤0.1. When d is within the above range, the positive electrode active material can have better structural stability and better electrochemical performance.
[0036] In some embodiments of the present application, f / (e+f)≤0.15. When f / (e+f) is within the above range, the positive electrode active material has an appropriate amount of anion doping, which can improve the cycle stability and specific capacity of the material.
[0037] In some embodiments of the present application, at least a portion of the surface of the lithium nickel cobalt manganese oxide and / or lithium nickel cobalt aluminum oxide is provided with a coating layer, and the coating layer includes a coating element, and the coating element contains at least one of Al, Ti, Zr, Ba, Zn, F, and P.
[0038] The present application also relates to a method for preparing a positive electrode active material, comprising the following steps:
[0039] Taking or preparing nickel-cobalt-manganese and / or nickel-cobalt-aluminum precursors;
[0040] The nickel-cobalt-manganese and / or nickel-cobalt-aluminum precursor is mixed with a lithium source, calcined, crushed, and sieved once to obtain the positive electrode active material.
[0041] The nickel-cobalt-manganese and / or nickel-cobalt-aluminum precursor refers to a hydroxide containing nickel, cobalt and manganese (or aluminum) elements.
[0042] In some embodiments of the present application, the nickel-cobalt-manganese and / or nickel-cobalt-aluminum precursors are directly mixed with a lithium source and calcined once, while in other embodiments, the nickel-cobalt-manganese and / or nickel-cobalt-aluminum precursors may be pretreated to obtain nickel-cobalt-manganese and / or nickel-cobalt-aluminum oxides and then mixed with a lithium source and calcined once.
[0043] In some embodiments of the present application, the preparation method of nickel-cobalt-manganese and / or nickel-cobalt-aluminum precursors may be a coprecipitation method, wherein soluble salts of nickel, cobalt, manganese (or aluminum) are mixed with a precipitant and a complexing agent to react to obtain nickel-cobalt-manganese and / or nickel-cobalt-aluminum precursors. The soluble salts of nickel, cobalt, and manganese (or aluminum) include, but are not limited to, at least one of halides, sulfates, and nitrates of nickel-cobalt-manganese and / or nickel-cobalt-aluminum, the precipitant includes, but is not limited to, at least one of sodium hydroxide, potassium hydroxide, sodium bicarbonate, and ammonium carbonate, and the complexing agent includes, but is not limited to, at least one of ammonia water, ethylenediaminetetraacetate, and tartaric acid. The various raw materials may be formulated, for example, according to the proportions of the various elements in the positive electrode active material.
[0044] In some embodiments of the present application, the pH of the reaction system is controlled between 10 and 12, for example, it can be 10, 10.5, 11, 11.5, 12, and further controlled between 11 and 12, 11.2 and 11.8.
[0045] In some embodiments of the present application, the concentration of the complexing agent is 1 to 15 mol / L, further 1 to 10 mol / L, 2 to 5 mol / L.
[0046] In some embodiments of the present application, the reaction temperature is 40-80°C, further 40-60°C, 45-55°C.
[0047] In some embodiments of the present application, the prepared nickel-cobalt-manganese and / or nickel-cobalt-aluminum precursor is subjected to a primary heat treatment to remove free water on the surface of the precursor to obtain a preliminary heat treatment product. Further, the primary heat treatment temperature can be 50-100°C, 60-100°C, 70-100°C, 80-100°C, or 90-100°C.
[0048] In some embodiments of the present application, the product of the primary heat treatment is subjected to secondary heat treatment to remove hydroxide to obtain nickel-cobalt-manganese and / or nickel-cobalt-aluminum hydroxide. Further, the temperature of the secondary heat treatment can be 400-600° C., 500-600° C., 500-550° C. In some of the embodiments, after the secondary heat treatment, the nickel-cobalt-manganese and / or nickel-cobalt-aluminum oxide is further washed and dried.
[0049] In some embodiments of the present application, after the nickel-cobalt-manganese and / or nickel-cobalt-aluminum precursor is mixed with the lithium source, the temperature of the primary calcination is 700-980°C.
[0050] Wherein, the lithium source includes but is not limited to at least one of lithium oxide, lithium phosphate, lithium acetate, lithium hydroxide, lithium carbonate, and lithium nitrate. In some embodiments, since other metal or non-metal elements are also doped in the positive electrode active material, other metal or non-metal element sources can be added during the process of mixing the nickel cobalt manganese and / or nickel cobalt aluminum precursor with the lithium source and calcining once. For example, the nickel cobalt manganese and / or nickel cobalt aluminum precursor is mixed with the lithium source and the Me source (if present) and the Z source (if present) and calcined once. The Me source and the Z source include but are not limited to at least one of oxides, hydroxides, Me salts (such as Me halides, carbonates, nitrates, oxalates, etc.), Me acid salts, Z salts (such as Z potassium salts, lithium salts, ammonium salts), and Z acid salts.
[0051] In some embodiments of the present application, the primary calcination temperature is 800-950°C.
[0052] In some embodiments of the present application, after the primary calcination, the product is further crushed and screened to obtain a primary calcined product. The primary calcined product may have a suitable particle size and particle size distribution and satisfy the U value relationship, so that it can be directly used as a positive electrode active material, or it may be re-mixed and secondary calcined in order to further coat other metals or non-metallic elements.
[0053] In some embodiments of the present application, the temperature of the secondary calcination is 400-550°C, further 400-500°C.
[0054] It should be noted that in the above preparation method, for positive electrode active materials with different elemental compositions and ratios, the morphology, particle size and distribution of the particles of the active substance can be regulated by controlling the temperature and time of the primary calcination, the specific crushing and screening process and specific parameters after calcination (for example, using closed-loop airflow crushing, semi-closed-loop airflow crushing and other airflow crushing processes, adjusting the air intake rate, feed rate, etc.; controlling the sieve hole size, screening times), and possible secondary calcination and time, and then adjusting its compaction density and conductivity, so that its U is kept within the above range.
[0055] The method for preparing the positive electrode active material provided in the present application has a simple process, is easy to implement, has a cost advantage, and can be applied in large-scale industrial production.
[0056] In a second aspect of the present application, a lithium-ion secondary battery is provided. The lithium-ion secondary battery includes a positive electrode plate. The positive electrode plate includes a current collector and a positive electrode active material layer located on the current collector. The positive electrode active material layer includes the aforementioned positive electrode active material.
[0057] In some embodiments, the positive electrode active material layer further includes at least one of a conductive agent and a binder. The conductive agent includes but is not limited to at least one of graphite, acetylene black, carbon black, carbon nanotubes, carbon fibers, etc. The binder includes but is not limited to at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), polyurethane (PU), polyvinyl alcohol (PVA), polyvinyl butyral (PVB), etc. The current collector includes but is not limited to metal foil (such as aluminum foil, silver foil, tin foil, iron foil, titanium foil, nickel foil, copper foil or at least one of the alloy foils of the above metals), metal mesh (such as aluminum mesh, silver mesh, tin mesh, iron mesh, titanium mesh, nickel mesh, copper mesh or at least one of the alloy meshes of the above metals).
[0058] In some embodiments of the present application, the positive electrode active material layer includes 70-99wt% of positive electrode active material, 0.5-6wt% of conductive agent and 0.5-20wt% of binder. Further, the mass fraction of the positive electrode active material in the positive electrode active material layer is 80-99wt%, 90-99wt%, 95-99wt%; the mass fraction of the conductive agent in the positive electrode active material layer is 1-6wt%, 2-5wt%; the mass fraction of the binder in the positive electrode active material layer is 1-10wt%, 1-5wt%.
[0059] In some embodiments of the present application, when the positive electrode active material, the conductive agent and the binder are made into the positive electrode active material layer, they are dispersed in a solvent and then coated on a positive electrode current collector and dried to obtain the positive electrode active material layer. For example, N-methylpyrrolidone (NMP) can be used as the solvent.
[0060] In some embodiments of the present application, a lithium-ion secondary battery includes a shell and an electrode assembly, wherein the shell accommodates the electrode assembly, and the electrode assembly includes a positive electrode sheet, a negative electrode sheet, and a separator located between the positive electrode sheet and the negative electrode sheet.
[0061] In some embodiments of the present application, the negative electrode plate includes but is not limited to a lithium plate, a negative electrode current collector having a negative electrode active material layer on its surface, etc. Similar to the positive electrode active material layer, the negative electrode active material layer includes a negative electrode active material, and in some embodiments, also includes a conductive agent and a binder.
[0062] In some embodiments of the present application, the negative electrode active material includes but is not limited to at least one of natural graphite, artificial graphite, mesophase microcarbon beads (MCMB), hard carbon, soft carbon, silicon, silicon-carbon composite, Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel structure lithium titanate, etc. The conductive agent, binder, and negative electrode current collector can be selected from the same selection range as the conductive agent and binder in the above-mentioned positive electrode. Similarly, similar to the positive electrode, the negative electrode can be prepared by mixing the above-mentioned negative electrode active material, binder, and conductive agent and coating them on the current collector and drying them, and can further be prepared by rolling, cutting, and other processes.
[0063] In some embodiments of the present application, the electrolyte may be at least one of an electrolyte solution and a solid electrolyte, and preferably a conventional electrolyte solution may be used.
[0064] In some embodiments of the present application, the separator includes, but is not limited to, a single-layer or multi-layer film of one or more materials selected from the group consisting of polyethylene (PE), polypropylene (PP), and polyvinylidene fluoride (PVDF).
[0065] In some embodiments of the present application, the positive electrode sheet, the negative electrode sheet and the separator are obtained by at least one of winding, stacking, etc. to obtain an electrode assembly, and the electrode assembly is accommodated in a shell, which can be a soft shell or a hard shell. After the electrolyte is injected and sealed, a lithium-ion secondary battery is obtained.
[0066] It is understandable that the conductive agent, binder, electrolyte, and separator may also be made of other materials known in the art or by other methods.
[0067] In some embodiments of the present application, the lithium-ion secondary battery housing may be an aluminum-plastic film.
[0068] In some embodiments of the present application, the lithium-ion secondary battery housing may be a hard shell or a soft shell.
[0069] In some embodiments of the present application, a soft-shell battery (also referred to as a soft-pack battery) includes two large surfaces arranged opposite to each other, and the two large surfaces are the two surfaces with the largest areas in the soft-pack battery.
[0070] In some embodiments of the present application, during 4C rate charging, the maximum temperature rise of the shell ΔT≤50°C.
[0071] In some embodiments of the present application, when the shell is a hard shell, the maximum temperature rise ΔT at the center of the bottom of the hard shell battery is ≤50°C.
[0072] The bottom of the hard shell battery is arranged opposite to the top cover of the battery.
[0073] In some embodiments of the present application, when the shell is a soft shell, the maximum temperature rise ΔT of the center of the large surface of the soft shell battery is ≤50° C. The maximum temperature rise refers to the temperature difference between the maximum temperature that can be reached at a specific position and the original temperature condition (such as room temperature) during rate charging.
[0074] According to a third aspect of the present application, an electrical device is provided, wherein the electrical device comprises the aforementioned lithium-ion secondary battery.
[0075] Among them, electrical equipment refers to any equipment that can use electrical energy and convert it into mechanical energy, thermal energy, light energy or other one or more forms of energy, such as electric motors, electric heat engines, electric light sources, etc. Specifically, it can include but is not limited to mobile devices, electric vehicles, electric trains, ships and satellites, energy storage systems, etc. Mobile devices can be mobile phones, laptops, drones, sweeping robots, electronic cigarettes, etc.; electric vehicles can be pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.
[0076] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0077] Figure 1 This is a scanning electron microscope image of the positive electrode active material provided in Example 1 of the present application.
[0078] Figure 2 This is a scanning electron microscope image of the positive electrode active material provided in Comparative Example 1 of the present application.
[0079] Figure 3 These are the results of the gram capacity test of the positive electrode active materials of Example 1 and Comparative Example 1 of the present application.
[0080] Figure 4 It is the direct current resistance DCR of the positive electrode active materials of Example 1 and Comparative Example 1 of the present application in the room temperature power test.
[0081] Figure 5 It is the DC resistance DCR of the low temperature power test of the positive electrode active materials of Example 1 and Comparative Example 1 of the present application.
[0082] Figure 6 It is the capacity retention rate of the positive electrode active materials of Example 1 and Comparative Example 1 of the present application under different rate conditions.
[0083] Figure 7 These are the room temperature fast charge cycle test results of the positive electrode active materials of Example 1 and Comparative Example 1 of the present application. DETAILED DESCRIPTION
[0084] The following will clearly and completely describe the concept of the present application and the technical effects produced in combination with the embodiments, so as to fully understand the purpose, features and effects of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of them. Based on the embodiments of the present application, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present application.
[0085] The embodiments of the present application are described in detail below. The described embodiments are exemplary and are only used to explain the present application, and should not be understood as limiting the present application.
[0086] In the description of this application, "several" means more than one, "more" means more than two, "greater than", "less than", "exceed", etc. are understood to exclude the number itself, and "above", "below", "within", etc. are understood to include the number itself. If there is a description of "first" or "second", it is only used for the purpose of distinguishing technical features, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features.
[0087] In the description of the present application, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0088] Example 1
[0089] This embodiment provides a method for preparing a positive electrode active material, comprising the following steps:
[0090] (1) Add nickel sulfate, cobalt sulfate and manganese sulfate to deionized water to prepare a nickel-cobalt-manganese sulfate solution, wherein the molar ratio of nickel, cobalt and manganese elements in the nickel-cobalt-manganese sulfate solution is Ni:Co:Mn=60:10:30. Add 2 mol / L ammonia solution and 8 mol / L sodium hydroxide solution to the solution at a uniform speed and in parallel, wherein the ammonia solution contains 0.6% tetraethylammonium hydroxide by mass, and the pH is controlled between 11.2 and 11.8 by sodium hydroxide. Nitrogen protection is used during the reaction, the stirring speed is 500 rpm and the temperature of the reaction device is about 50°C, and the reaction time is controlled to obtain a ternary precursor Ni 0.6 Co 0.1 Mn 0.3 (OH)2.
[0091] (2) The ternary precursor is placed in a hot air circulation drying oven and subjected to a primary heat treatment at 95°C for 2 hours to obtain a preliminary heat-treated product, and then transferred to a calcining furnace and subjected to a secondary heat treatment at 510°C for 5 hours to obtain a high-temperature product, which is then washed and dried to obtain the ternary precursor oxide.
[0092] (3) According to the ratio of the relevant elements in the molecular formula, the ternary precursor oxide, lithium carbonate, strontium carbonate SrCO3, zirconium oxide ZrO2, and tungsten oxide WO3 are added to the mixer and mixed. The mixed materials are placed in a tube furnace and heated to 935°C at 5°C / min in an oxygen atmosphere for 12 hours. The materials are cooled to room temperature with the furnace, and the average particle size D is obtained by air flow crushing and classification. v 50 is a precursor of active material particles of 3.8 μm.
[0093] (4) The precursor of the active material particles is coated with aluminum oxide Al2O3 and titanium oxide TiO2 and then returned to the furnace for secondary calcination at a calcination temperature of 450°C. After screening, the positive electrode active material C1 is obtained. The molecular formula of C1 is Li(Ni 0.6 Co 0.1 Mn 0.3 ) 0.995 Sr 0.001 Zr 0.003 W 0.001 O2.
[0094] Test Method
[0095] 1. Morphology: Scanning electron microscope (SEM) was used to test the microscopic morphology of the positive electrode active material C1.
[0096] 2. Particle size: Use a laser particle size analyzer to test the particle size distribution of the positive electrode active material C1. v 50 and D v 99.
[0097] 3. Conductivity and compaction density: Mitsubishi MCP-PD51 powder resistivity meter is used to test the powder volume resistivity and compaction density of the positive electrode active material under a pressure of 60MPa. The positive electrode active material powder is added to the sample table, and a 60MPa pressure is applied to the powder by a press. After the pressure stabilizes, the powder volume resistivity ρ and the compaction density C of the positive electrode active material under a pressure of 60MPa can be read from the resistivity meter. The powder conductivity is converted by K=1 / ρ.
[0098] The morphology test results are as follows Figure 1 As shown in the figure, it can be seen that there are a large number of monodisperse primary particles with uniform morphology, compact structure and uniform distribution, and there are also certain secondary particles formed by the agglomeration of primary particles.
[0099] According to the measured particle size, conductivity and compaction density of the positive electrode active material C1, the U of C1 is calculated to be 1.29. The specific parameters are shown in Table 1.
[0100] This embodiment also provides a lithium-ion secondary battery made of the positive electrode active material, comprising the following steps:
[0101] 1. Preparation of positive electrode
[0102] The positive electrode active material prepared above, the conductive carbon black SP and the binder PVDF were dispersed in the solvent NMP in a mass ratio of 96:3:1 and mixed evenly to obtain a positive electrode slurry.
[0103] The positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil, and the positive electrode sheet is obtained after baking, cold pressing and cutting.
[0104] 2. Preparation of negative electrode sheet
[0105] Graphite, conductive carbon black SP and binder PVDF were dispersed in solvent deionized water in a mass ratio of 95.7:1:3.3 and mixed evenly to obtain a negative electrode slurry.
[0106] The negative electrode slurry is evenly coated on the negative electrode current collector copper foil, and the negative electrode sheet is obtained after baking, cold pressing and cutting.
[0107] 3. Preparation of Electrolyte
[0108] Ethylene carbonate (EC), dimethyl carbonate (DMC) and propylene carbonate (PC) are mixed uniformly in a mass ratio of 40:30:30 to obtain an organic solvent. LiPF6 is dissolved in the organic solvent and mixed uniformly to obtain an electrolyte solution, wherein the content of LiPF6 is 12.5% based on the mass of the electrolyte solution.
[0109] 4. Preparation of soft pack batteries
[0110] The positive electrode sheet, PP / PE / PP composite isolation film and negative electrode sheet are stacked and wound in sequence, the roll core is placed in an aluminum-plastic film for welding and baking, and the above-mentioned electrolyte is added and sealed to complete the preparation of the soft-pack battery.
[0111] Example 2
[0112] This embodiment provides a positive electrode active material, which is different from the embodiment 1 in the following aspects:
[0113] ① In step 1, the molar ratio of nickel, cobalt and manganese is adjusted so that the ternary precursor of the positive electrode active material is Ni 0.63 Co 0.08 Mn 0.29 (OH)2.
[0114] ② In step 3, the Me source for the preparation of the positive electrode active material is only strontium carbonate, and the added amount is such that the ratio of the molar amount of strontium element to the total molar amount of nickel element, cobalt element and manganese element in the active material particles is 0.0012:0.9988, and the ratio of the molar amount of lithium element to the total molar amount of nickel, cobalt, manganese and strontium elements is 1.06:1.
[0115] ③ In step 3, the primary calcination temperature is adjusted from 935°C to 925°C.
[0116] In the positive electrode active material C2 finally prepared in this embodiment, the molecular formula of the lithium nickel cobalt manganese oxide particles is Li(Ni 0.63 Co 0.08 Mn 0.29 ) 0.9988 Sr 0.0012 O2.
[0117] According to the measured particle size, conductivity and compaction density of the positive electrode active material C2, the U of C2 is calculated to be 3.31. The specific parameters are shown in Table 1.
[0118] Example 3
[0119] This embodiment provides a positive electrode active material, which is different from the embodiment 1 in the following aspects:
[0120] ① In step 1, the molar ratio of nickel, cobalt and manganese is adjusted so that the ternary precursor of the positive electrode active material is Ni 0.63 Co 0.09 Mn 0.28 (OH)2.
[0121] ② In step 3, the primary calcination temperature was adjusted from 935°C to 930°C, and the calcination time was adjusted from 12h to 13h.
[0122] In the positive electrode active material C3 finally prepared in this embodiment, the molecular formula of the lithium nickel cobalt manganese oxide particles is Li(Ni 0.63 Co 0.09 Mn 0.28 ) 0.997 Sr 0.001 Zr 0.001 W 0.001 O2.
[0123] According to the measured particle size, conductivity and compaction density of the positive electrode active material C3, the U of C3 is calculated to be 1.69. The specific parameters are shown in Table 1.
[0124] Example 4
[0125] This embodiment provides a positive electrode active material, which is different from the embodiment 1 in the following aspects:
[0126] ① In step 1, the molar ratio of nickel, cobalt and manganese is adjusted so that the ternary precursor of the positive electrode active material is Ni 0.65 Co 0.05 Mn 0.30 (OH)2.
[0127] ② In step 3, the primary calcination temperature was adjusted from 935°C to 940°C, and the calcination time was adjusted from 12h to 13.5h.
[0128] In the positive electrode active material C4 finally prepared in this embodiment, the molecular formula of the lithium nickel cobalt manganese oxide particles is Li(Ni 0.65 Co 0.05 Mn 0.3 ) 0.997 Sr 0.001 Zr 0.001 W 0.001 O2.
[0129] According to the measured particle size, conductivity and compaction density of the positive electrode active material C4, the U of C4 is calculated to be 0.59. The specific parameters are shown in Table 1.
[0130] Example 5
[0131] This embodiment provides a positive electrode active material, which is different from the embodiment 1 in the following aspects:
[0132] ① In step 1, the molar ratio of nickel, cobalt and manganese is adjusted so that the ternary precursor of the positive electrode active material is Ni 0.68 Co 0.07 Mn 0.25 (OH)2.
[0133] ② In step 3, the primary calcination temperature was adjusted from 935°C to 930°C, and the calcination time was adjusted from 12h to 14h.
[0134] In the positive electrode active material C5 finally prepared in this embodiment, the molecular formula of the lithium nickel cobalt manganese oxide particles is Li(Ni 0.68 Co 0.07 Mn 0.25 ) 0.997 Sr 0.001 Zr 0.001 W 0.001 O2.
[0135] According to the measured particle size, conductivity and compaction density of the positive electrode active material C5, the U of C5 is calculated to be 0.44. The specific parameters are shown in Table 1.
[0136] Example 6
[0137] This embodiment provides a positive electrode active material, which is different from the embodiment 1 in the following aspects:
[0138] ① In step 4, the temperature of the secondary calcination is adjusted from 450°C to 400°C.
[0139] In the positive electrode active material C6 finally prepared in this embodiment, the molecular formula of the lithium nickel cobalt manganese oxide particles is Li(Ni 0.6 Co 0.1 Mn 0.3 ) 0.995 Sr 0.001 Zr 0.003 W 0.001 O2.
[0140] According to the measured particle size, conductivity and compaction density of the positive electrode active material C6, the U of C6 is calculated to be 2.97. The specific parameters are shown in Table 1.
[0141] Example 7
[0142] This embodiment provides a positive electrode active material, which is different from the embodiment 1 in the following aspects:
[0143] ① In step 4, the temperature of the secondary calcination is adjusted from 450°C to 550°C.
[0144] In the positive electrode active material C7 finally prepared in this embodiment, the molecular formula of the lithium nickel cobalt manganese oxide particles is Li(Ni 0.6 Co 0.1 Mn 0.3 ) 0.995 Sr 0.001 Zr 0.003 W 0.001 O2.
[0145] According to the measured particle size, conductivity and compaction density of the positive electrode active material C7, the U of C7 is calculated to be 1.72. The specific parameters are shown in Table 1.
[0146] Example 8
[0147] This embodiment provides a positive electrode active material, which is different from the embodiment 1 in the following aspects:
[0148] ① In step 3, the Me source for the preparation of the positive electrode active material is only zirconium oxide, and the added amount is such that the ratio of the molar amount of zirconium element to the total molar amount of nickel element, cobalt element and manganese element in the active material particles is 0.003:0.997, and the ratio of the molar amount of lithium element to the total molar amount of nickel, cobalt, manganese and strontium elements is 1.06:1.
[0149] ② In step 3, the primary calcination temperature was adjusted from 935°C to 930°C, and the calcination time was adjusted from 12h to 13h.
[0150] In the positive electrode active material C8 finally prepared in this embodiment, the molecular formula of the lithium nickel cobalt manganese oxide particles is Li(Ni 0.6 Co 0.1 Mn 0.3 ) 0.997 Zr 0.003 O2.
[0151] According to the measured particle size, conductivity and compaction density of the positive electrode active material C8, the U of C8 is calculated to be 1.46. The specific parameters are shown in Table 1.
[0152] Example 9
[0153] This embodiment provides a positive electrode active material, which is different from the embodiment 1 in the following aspects:
[0154] ① Adjust the ratio of nickel, cobalt and manganese in step 1.
[0155] ② In step 3, without doping Me source, lithium and nickel, cobalt and manganese are directly mixed and reacted in a molar ratio of 1.06:1, and air flow crushing is performed by controlling the air flow velocity, feed rate, etc. The product obtained after classification is directly used as the positive electrode active material C9 without secondary calcination.
[0156] The molecular formula of the lithium nickel cobalt manganese oxide particles in the positive electrode active material C9 is LiNi 0.7 Co 0.2 Mn 0.1 O2.
[0157] According to the measured particle size, electrical conductivity and compaction density of the positive electrode active material C9, U of C9 was calculated to be 2.10.
[0158] Example 10
[0159] This embodiment provides a positive electrode active material, which is different from the embodiment 1 in the following aspects:
[0160] ① In step 3, without the doped Me source, lithium and nickel, cobalt and manganese are directly mixed and reacted in a molar ratio of 1.1:1.
[0161] ② In step 4, the precursor of the active material particles is mixed with magnesium fluoride and then returned to the furnace for secondary calcination at 450°C for 5 hours, and the positive electrode active material C10 is obtained after screening. The molecular formula of the particles of lithium nickel cobalt manganese oxide in the positive electrode active material C10 is Li 1.04 Ni 0.6 Co 0.1 Mn 0.3 O2.
[0162] According to the measured particle size, conductivity and compaction density of the positive electrode active material C10, U of C10 was calculated to be 3.44.
[0163] Embodiment 11
[0164] This embodiment provides a positive electrode active material, which is different from the embodiment 1 in the following aspects:
[0165] ① In step 3, the ternary precursor oxide, lithium carbonate, lithium fluoride, aluminum oxide, and boron oxide are added to the mixer for mixing reaction according to the relevant ratio in the molecular formula. Active material particles are obtained by adjusting the air intake speed, feed speed, screening conditions, etc., as the positive electrode active material C11.
[0166] The molecular formula of the lithium nickel cobalt manganese oxide particles in the positive electrode active material C11 is Li(Ni 0.6 Co 0.1 Mn 0.3 ) 0.998 Al 0.001 B 0.001 O 1.994 F 0.006 .
[0167] According to the measured particle size, conductivity and compaction density of the positive electrode active material C11, the U of C11 was calculated to be 1.83.
[0168] Example 12
[0169] This embodiment provides a positive electrode active material, which is different from the embodiment 1 in the following aspects:
[0170] ① In step 3, the ternary precursor oxide, lithium carbonate, tungsten oxide, and titanium oxide are added to the mixer for mixing reaction according to the relevant ratio in the molecular formula. Active material particles are obtained by adjusting the air intake speed, feed speed, screening conditions, etc., as the positive electrode active material C12.
[0171] The molecular formula of the particles of lithium nickel cobalt manganese oxide in the positive electrode active material C12 is Li(Ni 0.6 Co 0.1 Mn 0.3 ) 0.996 W 0.003 Ti 0.001 O2.
[0172] According to the measured particle size, conductivity and compaction density of the positive electrode active material C12, the U of C12 was calculated to be 4.41.
[0173] Example 13
[0174] This embodiment provides a positive electrode active material, which is different from Embodiment 12 in the following aspects:
[0175] ① In step 3, the ternary precursor oxide, lithium carbonate, tungsten oxide, and lithium fluoride are added to the mixer for mixing reaction according to the relevant ratio in the molecular formula. Active material particles are obtained by adjusting the air intake speed, feed speed, screening conditions, etc., as the positive electrode active material C13.
[0176] The molecular formula of the particles of lithium nickel cobalt aluminum oxide in the positive electrode active material C13 is Li(Ni 0.6 Co 0.1 Mn 0.3 ) 0.996 W 0.004 O 1.998 F 0.002 .
[0177] According to the measured particle size, conductivity and compaction density of the positive electrode active material C13, the U of C13 was calculated to be 2.39.
[0178] Comparative Example 1
[0179] This comparative example provides a positive electrode active material, which is different from Example 1 in the following aspects:
[0180] ① In step 3, the primary calcination temperature is adjusted from 935°C to 950°C.
[0181] ② In step 4, the temperature of the secondary calcination is adjusted from 450°C to 500°C.
[0182] In the positive electrode active material D1 finally prepared in this embodiment, the molar ratio of various elements such as nickel, cobalt and manganese is consistent with that of the positive electrode active material C1 in Example 1.
[0183] The test results of the microstructure of the positive electrode active material D1 are as follows: Figure 2 As shown in the figure, it can be seen that there are also a large number of monodisperse primary particles with uniform morphology, compact structure and uniform distribution, as well as a certain amount of agglomerated secondary particles.
[0184] However, according to the measured particle size, conductivity and compaction density of the positive electrode active material D1, the U of D1 is calculated to be 0.36, which does not meet the predetermined range. Specific parameters are shown in Table 1.
[0185] Comparative Example 2
[0186] This comparative example provides a positive electrode active material, which is different from Example 1 in the following aspects:
[0187] ① In step 3, the primary calcination temperature is adjusted from 935°C to 980°C.
[0188] ② In step 4, the temperature of the secondary calcination is adjusted from 450°C to 550°C.
[0189] In the positive electrode active material D2 finally prepared in this embodiment, the molar ratio of various elements such as nickel, cobalt and manganese is consistent with that of the positive electrode active material C1 in Example 1.
[0190] However, according to the measured particle size, conductivity and compaction density of the positive electrode active material D2, the U of D2 is calculated to be 0.17, which does not meet the predetermined range. Specific parameters are shown in Table 1.
[0191] Comparative Example 3
[0192] This comparative example provides a positive electrode active material, which is different from Example 1 in the following aspects:
[0193] ② In step 3, the only Me source for the preparation of the positive electrode active material is strontium carbonate, and the amount added is such that the ratio of the molar amount of strontium element to the total molar amount of nickel element, cobalt element and manganese element in the active material particles is 0.003:0.997, and the ratio of the molar amount of lithium element to the total molar amount of nickel, cobalt, manganese and strontium elements is 1:1.
[0194] ② In step 3, the primary calcination temperature was adjusted from 935°C to 900°C, and the calcination time was adjusted from 12h to 13h.
[0195] ③ In step 4, the temperature of the secondary calcination is adjusted from 450°C to 350°C.
[0196] In the positive electrode active material D3 finally prepared in this embodiment, the molar ratio of nickel, cobalt and manganese is consistent with that of the positive electrode active material C1 in Example 1, and the molar ratio of nickel, cobalt and manganese to lithium and the doping element is different from that in Example 1.
[0197] According to the measured particle size, conductivity and compaction density of the positive electrode active material D3, the U of D3 is calculated to be 5.64, which does not meet the predetermined range. The specific parameters are shown in Table 1.
[0198] Battery performance test method
[0199] 1. Gram capacity test of positive electrode active materials
[0200] At 25°C, the soft-pack battery was charged at a constant current of 0.33C to 4.35V, then charged at a constant voltage to a current less than or equal to 0.05C, then left for 5 minutes, and then discharged at a constant current of 0.33C to 2.8V. The discharge capacity at this time was the initial gram capacity.
[0201] 2. Lithium-ion battery power performance test
[0202] 2.1 Normal temperature power test
[0203] At 25°C, the soft-pack battery was charged to 4.35V at a constant current of 0.33C, and then charged at a constant voltage until the current was less than or equal to 0.05C. After that, the soft-pack battery was discharged at a constant current of 0.33C to adjust the charge state (SOC) of 90%, 50% and 20%, respectively. Then, the battery was discharged at 5C for 10s at SOC of 90%, 50% and 20%, respectively, and the voltage drop before and after discharge was recorded. The ratio of the voltage drop before and after discharge to the discharge current is the DC resistance DCR of the battery, and the DC resistance DCR of 90%, 50% and 20% was obtained respectively.
[0204] 2.2 Low temperature power test
[0205] At 25°C, the soft-pack battery was charged to 4.35V at a constant current of 0.33C, and then charged at a constant voltage until the current was less than or equal to 0.05C. After that, the soft-pack battery was discharged at a constant current of 0.33C to adjust the state of charge (SOC) of 90%, 50% and 20%, respectively. After adjusting the SOC, the temperature was adjusted to -20°C, and then discharged at 0.36C for 10s under SOC of 90%, 50% and 20%, respectively. The voltage drop before and after discharge was recorded, and the ratio of the voltage drop before and after discharge to the discharge current was calculated to obtain the DC resistance DCR of 90%, 50% and 20%, respectively.
[0206] 2.3 Lithium-ion battery charging rate performance test
[0207] At 25°C, the soft-pack battery was discharged at a constant current of 0.33C to 2.8V, and then charged at different constant current rates (0.2C / 0.3C / 0.5C / 1C / 1.5C / 2C / 3C / 4C) to 4.35V. Taking the capacity at 0.2C as 100%, the ratios of the charging capacity at other rates to the charging capacity at 0.2C were calculated in sequence to obtain the charging capacity retention rate after the rate was increased.
[0208] 2.4 Lithium-ion battery room temperature fast charge cycle test
[0209] At 25°C, the soft-pack battery is charged to 10% SOC at a constant current of 1C, then charged to 80% SOC at an equivalent constant current of 3C, then charged to 90% SOC at a constant current of 1C, then charged to 97% SOC at a rate of 0.5C, and finally discharged to 2% SOC at a constant current of 1C. This is a charge and discharge cycle, and the discharge capacity is recorded as the discharge capacity of the first cycle. The soft-pack battery is subjected to a fast charge and discharge cycle test according to the above method, and the discharge capacity of each cycle is recorded. The test is stopped when the capacity retention rate is lower than 80%. The cycle capacity retention rate (%) = discharge capacity of the nth cycle / discharge capacity of the first cycle × 100%.
[0210] The test results of various embodiments and comparative examples are shown in Table 1 and Table 2.
[0211] Table 1. Test results of relevant parameters of the embodiments and comparative examples
[0212]
[0213] Table 2. Performance test results of the embodiments and comparative examples
[0214]
[0215]
[0216] Among them, the maximum temperature rise during fast charging (℃) refers to the maximum temperature rise at the center of the large surface of the soft-pack battery during 4C rate charging.
[0217] The U value of comparative example 1 is less than 0.42, and K<180μs / cm, D v 99>14μm, C is between 3.1 and 3.7μm. Comparing the SEM images of Comparative Example 1 and Example 1, the particle size of the lithium nickel cobalt manganese oxide in Comparative Example 1 is significantly larger and more rounded, which can also be confirmed by the particle size measured by the laser particle size analyzer in Table 1. Compared with Example 1, D v 50 increased by 2.3μm, D v 99 increased by 4.3μm.
[0218] Comparing the 0.33C discharge capacity of Comparative Example 1 with that of Example 1, the results are as follows Figure 3 As shown in Table 2, the first discharge capacity in Comparative Example 1 is 8.6 mAh / g lower than that in Example 1.
[0219] Comparison of power performance at room temperature and low temperature Figure 4 , Figure 5 As shown in Table 2, the room temperature power performance of Comparative Example 1 is 30.5% worse than that of Example 1, and the low temperature power performance is 53.6% worse.
[0220] Comparing the capacity retention rates of Example 1 and Comparative Example 1 at high rates, the results are as follows Figure 6 As shown in Table 2, it can be seen that with the increase of the rate, the capacity retention rates of Example 1 and the comparative example are constantly decreasing, but it is obvious that the decrease in Comparative Example 1 is higher. Among them, at a rate of 4C, the capacity retention rate of Comparative Example 1 is reduced by 12.1% compared with that of Example 1.
[0221] Comparing the fast charge cycle performance of Example 1 and Comparative Example 1, the results are as follows Figure 7As shown in the figure, with the continuous increase in the number of cycles, the capacity retention rate of comparative example 1 decreases more significantly, reaching the test termination condition of 80% capacity retention rate at 1730 cycles, while Example 1 reaches 80% capacity retention rate at 2820 cycles. Therefore, compared with comparative example 1, the fast charging cycle performance of Example 1 is significantly improved.
[0222] In addition, combined with the data in Table 2, the U value of Comparative Example 2 is also less than 0.42, and K<180μs / cm, D v 99>14μm, C<3.1μm. It can be seen that the gram capacity, room temperature and low temperature power, high rate capacity retention rate and fast charge cycle performance are worse than those of comparative example 1. The reason is that the particles of lithium nickel cobalt manganese oxide, the positive electrode active material finally prepared in comparative example 2, have poor kinetics and high temperature rise, which further aggravates the side reactions and reduces the fast charge cycle life.
[0223] The U value of comparative example 3 is much greater than 4.50, K>430μs / cm, D v 99<8μm, C between 3.1 and 3.7μm, and D v 50 is also smaller than that of Example 1. Therefore, the positive electrode active material prepared in Comparative Example 3 has too small particles of lithium nickel cobalt manganese oxide. Although the gram capacity, room temperature and low temperature power, and high rate capacity retention rate can reach the level of some embodiments, and the kinetic performance is excellent, the positive electrode material deteriorates the side reaction with the electrolyte during use, accelerates the capacity decay significantly, and the fast charge cycle performance is still low. However, due to the characteristics of the material itself, its impedance is low and the temperature rise is not obvious.
[0224] In Examples 1 to 8 and Examples 9 to 12, the cobalt content in the positive electrode active material is relatively low. By ensuring that the ratio of each element in the molecular formula satisfies the predetermined relationship, the positive electrode active material can have a relatively high structural stability. The U of the positive electrode active material particles meets the predetermined range, ensuring that the positive electrode sheet using the positive electrode active material has high lithium ion and electron transmission performance, so that the positive electrode active material has a high gram capacity and cycle life. As a result, the lithium-ion secondary battery using the positive electrode active material has a higher energy density, and at the same time has better power performance and rate performance, especially good fast charging cycle performance, which can meet the needs of the fast charging technology that is rapidly popularizing and developing.
[0225] The present application is described in detail above in conjunction with the embodiments, but the present application is not limited to the above embodiments, and various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present application. In addition, the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.
Claims
1. A positive electrode active material, characterized in that The positive electrode active material comprises at least one of lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide, and the positive electrode active material satisfies 0.42≤U≤4.50; Wherein U=6K / (π·D v 99 2 ·C), K is the electrical conductivity of the powder of the positive electrode active material under a pressure of 60 MPa, in μs / cm; D v 99 is the particle size corresponding to when the cumulative volume distribution percentage of the positive electrode active material reaches 99%, in μm; C is the compaction density of the positive electrode active material powder under a pressure of 60 MPa, in g / cm 3 ; Based on the total molar amount of metal elements except lithium in the positive electrode active material being 100%, the molar percentage of the cobalt element is no more than 25%.
2. The positive electrode active material according to claim 1, characterized in that The positive electrode active material satisfies at least one of the following (i) to (iii): (i) 180 μs / cm≤K≤430 μs / cm; (ⅱ)8 μm≤D v 99≤14 μm; (ⅲ)3.1 g / cm 3 ≤C≤3.7 g / cm 3 。 3. The positive electrode active material according to claim 1, characterized in that The positive electrode active material satisfies 2.5 μm≤D v 50≤6 μm, D v 50 is the particle size corresponding to when the cumulative volume distribution percentage of the positive electrode active material reaches 50%.
4. The positive electrode active material according to any one of claims 1 to 3, characterized in that The lithium nickel cobalt manganese oxide and / or lithium nickel cobalt aluminum oxide comprises a general formula of Li x Ni a Co b R c Me d O e Z f The compound Among them, 0.8≤x≤1.2, a+b+c+d=1, b≤0.25, d≤0.12, e≥1, e+f≤2, and a~f are not negative numbers; Me includes at least one of Al, Zr, Sr, Ti, B, Mg, Sn, W, Y, Ba, Nb, Mo, Ta, Si, La, Er, Nd, Gd, and Ce; Z includes at least one of P, S, N, F, Cl, Br, and I; R is selected from at least one of Mn and Al.
5. The positive electrode active material according to claim 4, characterized in that 0.55≤a≤0.7, 0.05≤b≤0.25, 0.09≤c≤0.
3.
6. The positive electrode active material according to claim 1, characterized in that At least part of the surface of the lithium nickel cobalt manganese oxide and / or the lithium nickel cobalt aluminum oxide is provided with a coating layer, and the coating layer includes a coating element, and the coating element includes at least one of Al, Ti, Zr, Ba, Zn, F, and P.
7. A lithium ion secondary battery, characterized in that The invention comprises a shell and an electrode assembly, wherein the shell accommodates the electrode assembly, the electrode assembly comprises a positive electrode sheet, the positive electrode sheet comprises a current collector and a positive electrode active material layer located on the current collector, and the positive electrode active material layer comprises the positive electrode active material according to any one of claims 1 to 6.
8. The lithium ion secondary battery according to claim 7, characterized in that: During 4C rate charging, the maximum temperature rise of the shell is ΔT≤50°C.
9. Electrical equipment, characterized in that: A lithium ion secondary battery comprising any one of claims 7 to 8.