A carbon / talc / non-precious metal honeycomb catalytic composite material and preparation method thereof
By preparing carbon/talc/non-noble metal honeycomb catalytic composite materials, the problems of insufficient surface reactivity and poor water resistance of the catalyst carrier material are solved, achieving efficient removal of VOCs and improving the stability of the catalyst.
Patent Information
- Application Number
- CN202211742457.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-30
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-12-30
AI Technical Summary
When existing catalysts catalyze the oxidation of volatile organic compounds (VOCs), they have problems such as insufficient surface reactivity of the carrier material, scarcity of precious metal resources, and poor water resistance, which affects the enrichment effect of low-concentration VOCs and the stability of the catalyst.
Using carbon/talc/non-noble metal honeycomb catalytic composite material, modified polystyrene composite microspheres are combined with talc and non-noble metal salts to form a catalyst with high specific surface area and hydrophobic properties to improve catalytic performance and water resistance.
It significantly improves the catalytic performance and water resistance of the catalyst, enhances the adsorption capacity of VOCs, prevents the poisoning failure of non-precious metal catalysts, and achieves efficient VOCs removal.
Smart Images

Figure HDA0004030329420000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalyst preparation, and in particular relates to a carbon / talc / non-precious metal honeycomb catalytic composite material for catalytically oxidizing volatile organic compounds (VOCs) and a preparation method thereof. Background Art
[0002] With the increasingly serious air pollution problem and the increasingly stringent standards of national environmental protection regulations, VOCs waste gas treatment has become a top priority for air pollution prevention and control in my country. At present, catalytic oxidation technology can convert VOCs pollutants into CO2 and H2O more thoroughly under the action of catalysts, and is considered to be one of the most effective methods for VOCs elimination. At present, the catalysts used in catalytic oxidation technology are mostly honeycomb cordierite as carriers and precious metals as active components. Cordierite has problems such as small specific surface area, low surface activity, and easy detachment of active components, and has poor enrichment effect on low-concentration VOCs. Precious metals have the disadvantages of high price, scarce resources, and easy sintering and deactivation at high temperature. In recent years, non-precious metal catalysts are mainly transition metal (such as: Mn, Ce, Co, Ni, etc.) oxides, which have the advantages of abundant resources and low prices and have gradually become a development trend, but have the disadvantage of poor water resistance. In order to solve the above problems, natural mineral materials have gradually attracted the interest of researchers. Talc is a natural flaky clay silicate mineral. The siloxane structure (Si-O-Si) on the crystal surface gives it excellent water resistance. The treated talc surface has a large number of active groups, which can greatly increase its surface reactivity. Summary of the invention
[0003] In view of the problems existing in the background technology, the present invention provides a method for preparing a carbon / talc / non-precious metal honeycomb catalytic composite material, aiming to improve the surface reaction activity of the catalyst carrier material or the water resistance of the non-precious metal active component.
[0004] The technical solution adopted by the present invention includes the following characteristic steps:
[0005] 1. First, prepare talc-modified polystyrene composite microspheres. Wash the talc-modified polystyrene composite microspheres prepared in step 1 for 4 to 6 times with a hydrofluoric acid solution having a mass percentage concentration of 3% to 8%, filter, and wash with deionized water until the pH value of the filtrate is 5 to 7; redisperse the obtained filter cake in a non-precious metal salt solution having a mass percentage concentration of 15% to 30%, immerse for 12 to 48 hours, and evaporate to dryness to obtain a polystyrene / talc / non-precious metal composite;
[0006] The talc-modified polystyrene composite microspheres are prepared by adding polystyrene microspheres (Zhongke Leiming (Beijing) Technology Co., Ltd.) and a cationic emulsifier to deionized water at the same time, forming micelles after high-speed shear emulsification for 30 to 60 minutes, then adding talc powder (fineness 10 μm, Guilin Guiguang Talc Development Co., Ltd.), continuing stirring for 1 to 3 hours, filtering, and obtaining a talc-modified polystyrene composite microsphere filter cake; the emulsifier is a cationic emulsifier, preferably dodecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, hexadecylpyridinium bromide or octadecylamine polyoxyethylene ether diquaternary ammonium salt. The mass ratio of polystyrene microspheres to deionized water is 0.1 to 0.4:1, the mass ratio of emulsifier to polystyrene microspheres is 0.02 to 0.15:1; and the mass ratio of talc powder to polystyrene microspheres is 0.1 to 0.3:1.
[0007] The non-precious metal salt solution is one of manganese nitrate solution, manganese chloride solution, manganese sulfate solution, cerium nitrate solution, cerium chloride solution, cerium sulfate solution, cobalt nitrate solution, cobalt chloride solution, cobalt sulfate solution, nickel nitrate solution, nickel chloride solution or nickel sulfate solution; the mass ratio of the non-precious metal oxide to the talc-modified polystyrene composite microspheres is 0.01-0.08 (theoretical value).
[0008] 3. Add the polystyrene / talc / non-precious metal composite and glycerol mixture obtained in step 2 into a vacuum mud kneader and repeat the mud kneading for 4 to 6 times, wherein the ratio of the total mass of glycerol to the composite is 0.05 to 0.1:1; place the mixture after vacuum mud kneading in a molding extruder to obtain a honeycomb adsorbent, and microwave dry it at 90°C to 120°C for 30 to 60 minutes; calcine the dried honeycomb adsorbent at 500°C to 600°C for 2 to 4 hours to obtain a carbon / talc / non-precious metal honeycomb catalytic material.
[0009] Carbon / talc / non-precious metal honeycomb catalytic composite materials are used for catalytic degradation of VOC gases.
[0010] Specifically: catalytic oxidation removal was performed using paraxylene as a simulated gas. The performance evaluation of the catalyst was carried out on a VOC adsorption and desorption reactor (VDRT-3000, Quzhou Ward Instrument Co., Ltd.). 1g of catalyst (40-60 mesh) and 4g of quartz sand (40-60 mesh) were mixed evenly and placed in a quartz tube (inner diameter 28mm). Under the conditions of relative humidity RH=80% and catalytic oxidation reaction temperature of 300°C, paraxylene was produced by bubbling nitrogen at room temperature, and high-purity air was used as the carrier gas. The concentration of paraxylene was controlled by adjusting the flow rates of the bubbling gas and the carrier gas, that is, the air flow rate was 450mL / min and the nitrogen flow rate was 30mL / min, so that the concentration of paraxylene was 5000mg / m 3The concentration of p-xylene was analyzed online by GC-2014 gas chromatograph.
[0011] The beneficial effects of the present invention are:
[0012] 1. The present invention uses flaky talc for loading to make it hydrophobic; uses dilute hydrofluoric acid solution to wash the talc-modified polystyrene composite microspheres to increase their reaction activity, which is beneficial to the adsorption and loading of non-precious metal ions of the active component, and greatly improves the catalytic performance of the material.
[0013] 2. The carbon / talc / non-precious metal honeycomb catalytic composite material prepared by the present invention has the characteristics of both carbon and talc. On the one hand, the carbon material and the modified talc have a large specific surface area, which improves the efficient adsorption performance of VOCs; on the other hand, the carbon material and the modified talc have a certain hydrophobicity, which improves the water resistance of the catalytic material to a certain extent and prevents the poisoning and failure of the non-precious metal catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is a comparison chart of the performance of the catalytic materials prepared in Example 4, Comparative Example 1 and Comparative Example 2. DETAILED DESCRIPTION
[0015] Example 1
[0016] 1. Add 1.0 kg of polystyrene microspheres with a particle size of 50 μm (Zhongke Leiming (Beijing) Technology Co., Ltd., the same below) and 0.05 kg of dodecyltrimethylammonium chloride to 10.0 kg of deionized water at the same time, form micelles after high-speed shear emulsification for 30 minutes, and then add 0.1 kg of talcum powder (fineness 10 μm, Guilin Guiguang Talc Development Co., Ltd., the same below), continue stirring for 1 hour, filter and dry to obtain talc-modified polystyrene composite microspheres;
[0017] 2. The talc-modified polystyrene composite microspheres prepared in step 1 were washed 4 times with a 3% hydrofluoric acid solution, filtered, and washed with deionized water until the pH value of the filtrate was 7; the obtained filter cake was redispersed in 0.15 kg of a 15% manganese nitrate solution, immersed for 48 hours, and evaporated to dryness to obtain a polystyrene / talc / non-precious metal manganese composite;
[0018] 3. Take 1.0 kg of the polystyrene / talc / non-precious metal manganese complex obtained in step 2 and 0.05 kg of glycerol mixture, add them into a vacuum mud kneader and repeat the mud kneading for 4 times, place the mixture after vacuum mud kneading in a molding extruder to obtain a honeycomb adsorbent, and microwave dry it at 90°C for 60 minutes; the dried honeycomb adsorbent is calcined at 600°C for 2 hours to obtain a carbon / talc / manganese dioxide honeycomb catalytic material.
[0019] Example 2
[0020] 1. Add 1.0 kg of polystyrene microspheres with a particle size of 100 μm and 0.15 kg of hexadecyltrimethylammonium bromide to 2.5 kg of deionized water at the same time, form micelles after high-speed shear emulsification for 50 minutes, then add 0.3 kg of talcum powder, continue stirring for 3 hours, filter and dry to obtain talc-modified polystyrene composite microspheres;
[0021] 2. The talc-modified polystyrene composite microspheres prepared in step 1 were washed 4 times with a hydrofluoric acid solution having a mass percentage concentration of 8%, filtered, and washed with deionized water until the pH value of the filtrate was 5; the obtained filter cake was redispersed in 0.36 kg of a cerium nitrate solution having a mass percentage concentration of 30%, immersed for 12 hours, and evaporated to dryness to obtain a polystyrene / talc / non-precious metal cerium composite;
[0022] 3. Take 1.0 kg of the polystyrene / talc / non-precious metal manganese complex obtained in step 2 and 0.1 kg of glycerol mixture, add them to a vacuum mud kneader and repeat the mud kneading for 6 times, place the mixture after vacuum mud kneading in a molding extruder to obtain a honeycomb adsorbent, and microwave dry it at 120°C for 30 minutes; the dried honeycomb adsorbent is calcined at 500°C for 4 hours to obtain a carbon / talc / cerium dioxide honeycomb catalytic material.
[0023] Example 3
[0024] 1. Add 1.0 kg of polystyrene microspheres with a particle size of 80 μm and 0.1 kg of hexadecylpyridinium bromide to 3.33 kg of deionized water at the same time, form micelles after high-speed shear emulsification for 45 minutes, then add 0.2 kg of talcum powder, continue stirring for 2 hours, filter and dry to obtain talc-modified polystyrene composite microspheres;
[0025] 2. Wash the talc-modified polystyrene composite microspheres obtained in step 1 for 5 times with a 6% hydrofluoric acid solution, filter, and wash with deionized water until the pH value of the filtrate is 6; redisperse the obtained filter cake in 0.40 kg of a 20% nickel nitrate solution, immerse for 30 hours, and evaporate to dryness to obtain a polystyrene / talc / non-precious metal nickel composite;
[0026] 3. Take 1.0 kg of the polystyrene / talc / non-precious metal manganese complex obtained in step 2 and 0.08 kg of glycerol mixture, add them into a vacuum mud kneader and repeat the mud kneading for 5 times. Place the mixture after vacuum mud kneading in a molding extruder to obtain a honeycomb adsorbent, and microwave dry it at 105°C for 45 minutes; calcine the dried honeycomb adsorbent at 550°C for 3 hours to obtain a carbon / talc / nickel oxide honeycomb catalytic material.
[0027] Example 4
[0028] 1. Add 1.0 kg of polystyrene microspheres with a particle size of 100 μm and 0.1 kg of octadecylamine polyoxyethylene ether diquaternary ammonium salt to 5.0 kg of deionized water at the same time, emulsify at high speed for 60 minutes to form micelles, then add 0.15 kg of talcum powder, continue stirring for 1.5 hours, filter and dry to obtain talc-modified polystyrene composite microspheres;
[0029] 2. The talc-modified polystyrene composite microspheres prepared in step 1 are washed 6 times with a 5% by mass hydrofluoric acid solution, filtered, and washed with deionized water until the pH value of the filtrate is 6; the obtained filter cake is redispersed in 0.20 kg of a 25% by mass cobalt nitrate solution, immersed for 24 hours, and evaporated to dryness to obtain a polystyrene / talc / non-precious metal cobalt composite;
[0030] 3. Take 1.0 kg of the polystyrene / talc / non-precious metal manganese complex obtained in step 2 and 0.07 kg of glycerol mixture, add them into a vacuum mud kneader and repeat the mud kneading for 5 times, place the mixture after vacuum mud kneading in a molding extruder to obtain a honeycomb adsorbent, and microwave dry it at 110°C for 30 minutes; the dried honeycomb adsorbent is calcined at 600°C for 3 hours to obtain a carbon / talc / cobalt tetroxide honeycomb catalytic material.
[0031] Comparative Example 1
[0032] 1. Add 1.0 kg of polystyrene microspheres with a particle size of 100 μm into 5.0 kg of deionized water, and form micelles after high-speed shear emulsification for 60 minutes, then add 0.15 kg of talcum powder, continue stirring for 1.5 hours, filter and dry to obtain talc-modified polystyrene composite microspheres;
[0033] 2. The talc-modified polystyrene composite microspheres prepared in step 1 are washed 6 times with a 5% by mass hydrofluoric acid solution, filtered, and washed with deionized water until the pH value of the filtrate is 6; the obtained filter cake is redispersed in 0.20 kg of a 25% by mass cobalt nitrate solution, immersed for 24 hours, and evaporated to dryness to obtain a polystyrene / talc / non-precious metal cobalt composite;
[0034] 3. Take 1.0 kg of the polystyrene / talc / non-precious metal manganese complex obtained in step 2 and 0.07 kg of glycerol mixture, add them into a vacuum mud kneader and repeat the mud kneading for 5 times, place the mixture after vacuum mud kneading in a molding extruder to obtain a honeycomb adsorbent, and microwave dry it at 110°C for 30 minutes; the dried honeycomb adsorbent is calcined at 600°C for 3 hours to obtain a carbon / talc / cobalt tetroxide honeycomb catalytic material.
[0035] Comparative Example 2
[0036] 1. Add 1.0 kg of polystyrene microspheres with a particle size of 100 μm and 0.1 kg of octadecylamine polyoxyethylene ether diquaternary ammonium salt to 5.0 kg of deionized water at the same time, emulsify at high speed for 60 minutes to form micelles, then add 0.15 kg of talcum powder, continue stirring for 1.5 hours, filter and dry to obtain talc-modified polystyrene composite microspheres;
[0037] 2. Re-dispersing the talc-modified polystyrene composite microspheres obtained in step 1 in 0.20 kg of a 25% mass percent cobalt nitrate solution, immersing for 24 hours, and evaporating to dryness to obtain a polystyrene / talc / non-precious metal cobalt composite;
[0038] 3. Take 1.0 kg of the polystyrene / talc / non-precious metal manganese complex obtained in step 2 and 0.07 kg of glycerol mixture, add them into a vacuum mud kneader and repeat the mud kneading for 5 times, place the mixture after vacuum mud kneading in a molding extruder to obtain a honeycomb adsorbent, and microwave dry it at 110°C for 30 minutes; the dried honeycomb adsorbent is calcined at 600°C for 3 hours to obtain a carbon / talc / cobalt tetroxide honeycomb catalytic material.
[0039] Performance Evaluation
[0040] Catalytic performance test: catalytic oxidation removal was carried out with paraxylene as the simulated gas. The performance evaluation of the catalyst was carried out on a VOC adsorption and desorption reactor (VDRT-3000, Quzhou Ward Instrument Co., Ltd.). 1g of catalyst (40 mesh ~ 60 mesh) and 4g of quartz sand (40 mesh ~ 60 mesh) were mixed evenly and placed in a quartz tube (inner diameter 28mm). Under the conditions of relative humidity RH = 80% and catalytic oxidation reaction temperature of 300°C, paraxylene was produced by bubbling nitrogen at room temperature, and high-purity air was used as the carrier gas. The concentration of paraxylene was controlled by adjusting the flow rate of the bubbling gas and the carrier gas, that is: the air flow rate was 450mL / min and the nitrogen flow rate was 30mL / min, so that the concentration of paraxylene was 5000mg / m 3 The concentration of p-xylene was analyzed online by GC-2014 gas chromatograph. The results are as follows: Figure 1 As shown, the catalytic effect of Example 4 is significantly higher than that of Comparative Example 1 and Comparative Example 2; the conversion rates of the catalysts of Examples 1-3 are higher than 96%.
Claims
1. Application of a carbon / talc / non-precious metal honeycomb catalytic composite material in catalytic degradation of VOC gas, characterized in that: (1) First, prepare talc-modified polystyrene composite microspheres: the preparation method of talc-modified polystyrene composite microspheres is as follows: polystyrene microspheres and emulsifiers are added to deionized water at the same time, and micelles are formed after high-speed shear emulsification for 30 to 60 minutes, and then talcum powder is added, and stirring is continued for 1 to 3 hours to obtain a talc-modified polystyrene composite microsphere; the mass ratio of the emulsifier to the polystyrene microspheres is 0.02 to 0.15:1; the mass ratio of the talcum powder to the polystyrene microspheres is 0.1 to 0.3:1; the emulsifier is a cationic emulsifier such as dodecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, hexadecylpyridinium bromide or octadecylamine polyoxyethylene ether diquaternary ammonium salt; The talc-modified polystyrene composite microspheres are washed with a hydrofluoric acid solution, filtered, and washed with deionized water until the pH value of the filtrate is 5-7, and the obtained filter cake is dispersed in a non-precious metal salt solution with a mass percentage concentration of 15%-30%, immersed for 12-48 hours, and evaporated to dryness to obtain a polystyrene / talc / non-precious metal composite; the non-precious metal salt solution is one of manganese nitrate solution, manganese chloride solution, manganese sulfate solution, cerium nitrate solution, cerium chloride solution, cerium sulfate solution, cobalt nitrate solution, cobalt chloride solution, cobalt sulfate solution, nickel nitrate solution, nickel chloride solution or nickel sulfate solution; the mass ratio of the non-precious metal oxide to the talc-modified polystyrene composite microspheres is 0.01-0.08; (2) Adding a mixture of polystyrene / talc / non-precious metal composite and glycerol into a vacuum kneader and repeatedly kneading for 4 to 6 times, placing the mixture after vacuum kneading into a molding extruder to obtain a honeycomb adsorbent, and microwave drying, and calcining the dried honeycomb adsorbent at 500°C to 600°C for 2 to 4 hours to obtain a carbon / talc / non-precious metal honeycomb catalytic material.
2. The use of the carbon / talc / non-precious metal honeycomb catalytic composite material in catalytic degradation of VOC gas according to claim 1, characterized in that: The microwave drying conditions in step (2) are 90° C. to 120° C. for 30 to 60 minutes.