A modified nano concave ball container and its preparation method and application

The one-step synthesis of carbon-based concave spherical nanomaterials solves the problems of low efficiency and poor selectivity of existing heavy metal adsorbents, achieves efficient adsorption of heavy metals and reduces toxicity, and the material structure is uniform and environmentally friendly.

CN115957721BActive Publication Date: 2024-10-25JINGDEZHEN CERAMIC UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211718082.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-29
Publication Date
2024-10-25
Estimated Expiration
2042-12-29

AI Technical Summary

Technical Problem

The existing heavy metal adsorbents have low efficiency, poor selectivity and poor adsorbent uniformity, resulting in low treatment efficiency of heavy metal contaminated wastewater and secondary pollution problems.

Method used

A one-step method is used to synthesize carbon-based concave spherical polymer nanomaterials with specific morphology. Nano-concave spheres are formed through aldol condensation reaction. The surface is loaded with sulfhydryl groups to form a nano-concave sphere container rich in active sites to improve the adsorption efficiency of heavy metals.

Benefits of technology

It achieves efficient adsorption of heavy metals such as Cr6+, with a maximum adsorption capacity of 1130 mg/g, and reduces highly toxic Cr6+ to low-toxic Cr3+ during the adsorption process. The material structure is uniform and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115957721B_ABST
    Figure CN115957721B_ABST
Patent Text Reader

Abstract

The invention discloses a modified nano concave sphere container and a preparation method thereof and an application thereof in adsorbing heavy metal micro-pollutants, belonging to the technical field of sewage treatment. The modified nano concave sphere container of the invention adopts a self-assembly method, and is etched by acetone solvent, so that the low oligomer fragments located in the core of the sphere are dissolved to form a cavity, and then the hollow nanosphere is collapsed to form a concave sphere, and the concave sphere is modified with a thiol group to obtain a modified nano concave sphere container; the modified nano concave sphere container is used as an adsorbent, and the modified nano concave sphere container is controlled by controlling the adsorption parameters to Cr 6+ The maximum adsorption capacity can reach 1130mg / g, Cd 2+ The maximum adsorption capacity of ions is close to 580 mg / g, As 3+ The maximum adsorption capacity is close to 150 mg / g. The modified nano concave sphere container is a polymer material, which is green and environmentally friendly, and provides a new method for nano container uptake of heavy metal micro-pollutants.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of heavy metal adsorption, and specifically relates to a modified nano concave sphere container and a preparation method thereof and application thereof in the adsorption of heavy metal micro-pollutants. Background Art

[0002] Heavy metals have the characteristics of irritation, target organ toxicity, carcinogenicity and immunotoxicity. Direct discharge of heavy metal-contaminated wastewater into water bodies will seriously affect human and ecological environmental safety. At present, the treatment of industrial heavy metal-contaminated wastewater mainly adopts physical and chemical methods, such as adsorption, membrane separation, chemical precipitation, electrochemical method, etc. Among them, chemical precipitation is mainly used for the treatment of industrial wastewater with high concentration. The concentration of heavy metals in the residual supernatant is high and there is a problem of secondary pollution of chemical sludge; membrane separation has the problems of expensive membrane components and membrane pollution, and the electrochemical method has the problems of excessive power consumption and electrode passivation. The adsorption method is relatively simple and has a low treatment cost. However, the existing heavy metal adsorbents have problems such as low efficiency, poor selectivity and poor adsorbent uniformity.

[0003] Prior art CN111111605A discloses a magnetic nano-adsorbent for heavy metal chromium and its preparation method and application. It includes the preparation of a magnetic nano-adsorbent for removing heavy metal chromium. The preparation of the nano-adsorbent is as follows: LaCl3·6H2O and H2NCSNH2 are added to a turbid liquid containing dissolved iron ions and ferrous ions, and hydrazine hydrate is added under temperature control and stirring to obtain a nano-material of sulfur-doped iron-lanthanum bimetallic oxide. However, the material synthesized by the prior art is impure and is a mixture with poor reproducibility; at the same time, the chromium removal efficiency is only about 60%, and the chromium adsorption efficiency is not disclosed.

[0004] Prior art CN110302742 A discloses a preparation method and application method of a selective heavy metal adsorption nanomaterial, which uses perlite as raw material, and sequentially undergoes preheating, expansion, cooling, and ball milling, and then mixes with dilute sulfuric acid, filters, heats and concentrates the filtrate, calcines, and ball mills. However, the prior art process is complex, requires repeated calcination, and has high energy consumption.

[0005] Prior art CN106179238A discloses a porous nanofiber that rapidly absorbs heavy metal ions and a preparation method thereof, wherein sodium alginate and carboxymethyl chitosan are used as raw materials, dissolved in water together with a polymer, a porogen, and a reinforcing agent, and nanofibers are obtained by electrostatic spinning technology, and then cross-linked and molded by calcium ions to obtain porous nanofibers for heavy metal ion extraction. In addition, the prior art adopts electrostatic spinning technology to prepare nanofibers in view of the problems such as small specific surface area of ​​ordinary fibers, low adsorption of heavy metal ions, and long time to reach adsorption equilibrium. However, the specific surface area data of nanofibers is not disclosed in the prior art embodiments, and the data of adsorption equilibrium time and adsorption amount of heavy metal ions are not provided with relevant figures for verification. Summary of the invention

[0006] 1. Problems to be solved

[0007] One of the purposes of the present invention is to provide an adsorbent with higher selectivity and adsorption efficiency for heavy metal ions and a preparation method and application thereof.

[0008] The second object of the present invention is to provide a method for treating Cr 6+ There are materials with ultra-high adsorption capacity, and the evidence in the present invention shows that during the adsorption process, the highly toxic Cr 6+ Reduced to low-toxic Cr 3+ ; In order to solve the problems of small specific surface area, unstable material morphology leading to poor repeatability, low adsorption capacity and efficiency of existing adsorbents, the present invention synthesizes carbon-based concave spherical polymers with specific morphology through a one-step method. The polymers have uniform morphology and are rich in functional groups such as carboxyl and amino groups on the surface, which help to provide active sites and thus increase their adsorption capacity. In particular, the cavity structure inside them helps them to act as nanocontainers to adsorb heavy metal pollutants.

[0009] 2. Technical solution

[0010] To solve the above problems, the present invention adopts the following technical solutions:

[0011] A modified nano concave ball container adopts a self-assembly method, uses 3-aminophenol and formaldehyde as raw materials, and uses ammonia water as a catalyst to form solid balls with different oligomerization levels through an aldol condensation reaction, and uses acetone as a solvent to dissolve oligomers with lower molecular weight to form a cavity structure. When the core-shell thickness is insufficient to support the cavity structure, collapse is formed to obtain bowl-shaped collapsed nano concave balls with a particle size of 300-500nm, wherein the thickness of the thick-edge core-shell is about 30nm, and the corresponding thin-edge core-shell thickness is about 15nm. The surface of the nano concave ball is smooth, and the diameter of the cavity is about 200nm. The surface of the modified nano concave ball container is loaded with thiol groups.

[0012] Preferably, the amount of thiol groups loaded on the surface of the modified nano concave sphere container is 5% to 15%.

[0013] Preferably, the specific surface area of ​​the modified nano concave sphere container is 1500 to 2200 m 2 / g.

[0014] The present invention further provides a method for preparing the modified nano concave sphere container according to any one of the above technical solutions, comprising the following steps:

[0015] 1) dissolving 3-aminophenol in water, adding formaldehyde and ammonia water to the solution, stirring to cause polymerization reaction;

[0016] 2) adding acetone to the system after the reaction in step 1), stirring, and continuing the reaction;

[0017] 3) Centrifuge to obtain a hollow concave sphere;

[0018] 4) The hollow concave spheres obtained in step 3) are modified with mercapto groups to obtain modified nano concave sphere containers.

[0019] Preferably, in step 1), the mass volume ratio (mg:mL) of 3-aminophenol to formaldehyde is (1-2):1; and / or

[0020] The polymerization reaction time in step 1) is 20 to 60 minutes; and / or

[0021] The volume ratio of water in step 1) to acetone in step 3) is (1-2):1.

[0022] Preferably, the method for modifying the thiol group in step 4) is: modifying the hollow concave spheres in step 3) using 4-aminothiophenol.

[0023] Preferably, the method for thiol modification in step 4) is specifically as follows: adding 4-aminothiophenol to a saturated NH4Cl buffer solution, gradually heating to 53°C while stirring to form a solution 1, and cooling in an ice bath; adding a NaNO2 solution dropwise to the solution 1 under continuous stirring, adding a hollow concave ball, and continuously stirring for 6 to 18 hours.

[0024] The present invention also provides an application of the modified nano concave sphere container in adsorbing heavy metal micropollutants, characterized in that the heavy metal micropollutants include As 3+ Cr 6+ 、Cd 2+ , Pb 2+ One or more heavy metal ions.

[0025] Preferably, the heavy metal micropollutants include heavy metal ions Cr 6+ .

[0026] Preferably, the concentration of the modified nano concave sphere container is 0.05-0.4 mg / mL.

[0027] Preferably, the concentration of the heavy metal ions is 10 to 100 mg / L, preferably 15 to 50 mg / L, and more preferably 20 to 30 mg / L.

[0028] Preferably, the pH suitable for the modified nano concave sphere container to adsorb heavy metal micropollutants is 1 to 9. 6+ The optimal pH range is 2-4; for Cd 2+ , the optimal pH range is 5-7; for As 3+, the optimal pH range is 5-7; for Pb 2+ , the optimal pH range is 5-7.

[0029] 3. Beneficial effects

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] (1) The modified nano concave sphere container of the present invention has a uniform structure and is resistant to heavy metal ions, especially Cr 6+ With a surprising adsorption capacity, Cr 6+ 、Cd 2+ 、As 3+ The maximum adsorption amounts can reach 1130mg / g, 580mg / g and 150mg / g respectively.

[0032] (2) The modified nano concave sphere container of the present invention has the following advantages: 6+ It has a very high adsorption capacity. During the adsorption process, the highly toxic Cr 6+ Converted into low-toxic Cr 3+ ,Cr 3+ It is also adsorbed by the nano concave ball container.

[0033] (3) The present invention is based on a heavy metal micro-pollutant adsorption method using a modified nano concave sphere container, wherein the modified nano concave sphere container is a carbon-based polymer material and is green and pollution-free to the environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 TEM and SEM images of the nano concave sphere container in Example 1.

[0035] Figure 2 is Cr under different pH conditions in Example 2 6+ 、Cd 2+ Adsorption amount.

[0036] Figure 3 For the adsorption of Cr in Example 2 6+ 、Cd 2+ XPS of the mixture (ac adsorption of Cr 6+ ; df adsorption Cd 2+ ).

[0037] Figure 4 Cr under the dosage conditions in Example 3 6+ 、Cd 2+ Adsorption amount and adsorption rate.

[0038] Figure 5 Cr in Example 4 6+ 、Cd 2+ Adsorption kinetics.

[0039] Figure 6 Cr in Example 5 6+ 、Cd 2+ Competitive adsorption.

[0040] Figure 7 Cr in Example 5 6+ 、Cd 2+ Competitive adsorption.

[0041] Figure 8 As in Example 5 3+ 、Cd 2+ Competitive adsorption.

[0042] Fig. 9 is As under different pH conditions in Example 6 3+ , Pb 2+ Adsorption amount and adsorption rate.

[0043] Fig.10 is As under different dosage conditions in Example 7 3+ , Pb 2+ Adsorption amount and adsorption rate.

[0044] Fig.11 As in Example 8 3+ , Pb 2+ Adsorption kinetics.

[0045] Fig.12 As in Example 9 3+ , Pb 2+ Competitive adsorption.

[0046] Fig.13 As in Example 9 3+ Cr 6+ Competitive adsorption. DETAILED DESCRIPTION

[0047] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs; the term "and / or" used herein includes any and all combinations of one or more of the associated listed items.

[0048] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased from the market.

[0049] As used herein, the term "about" is used to provide flexibility and imprecision associated with a given term, measurement or value. The degree of flexibility for a particular variable can be easily determined by one skilled in the art.

[0050] Concentration, amount and other numerical data can be presented in range format herein.It should be understood that such range format is only used for convenience and simplicity, and should be flexibly interpreted as not only including the numerical value clearly described as range limit, but also including all single numerical values ​​or sub-ranges contained in the range, just as each numerical value and sub-range are clearly described.For example, the numerical range of about 1 to about 4.5 should be interpreted as not only including the limit value of 1 to about 4.5 clearly described, but also including single numerals (such as 2,3,4) and sub-ranges (such as 1 to 3,2 to 4, etc.).The same principle is applicable to the scope of only narrating a numerical value, such as "less than about 4.5", which should be interpreted as including all the above-mentioned values ​​and ranges.In addition, no matter how the breadth of the described range or feature is, this explanation should be applicable.

[0051] The present invention is further described below in conjunction with specific embodiments and drawings.

[0052] Example 1

[0053] Raw materials: 3-aminophenol, formaldehyde, ammonia water, acetone.

[0054] The preparation method of the modified nano concave sphere container comprises the following steps:

[0055] 1) Dissolve 0.1 g of 3-aminophenol in 30 mL of water; add 0.1 mL of formaldehyde and 0.05 mL of ammonia water, stir; react for 20 min;

[0056] 2) Add 30 mL of acetone to the reaction system; stir and continue the reaction for 20 min;

[0057] 3) Centrifugal to obtain a hollow concave sphere;

[0058] 4) Thiol modification to obtain modified hollow concave spheres: 12 mmol 4-aminothiophenol was added to 15 mL saturated NH4Cl buffer solution, and the solution was gradually heated to 53°C while stirring to form solution 1, which was then cooled in an ice bath; 12 mmol NaNO2 solution (20 mL deionized water) was added dropwise to solution 1 under continuous stirring, 0.1 g of hollow concave spheres was added to the mixed solution, and stirring was continued for 12 h. The solution was centrifuged and collected to obtain modified nano concave spheres.

[0059] The prepared modified nano concave sphere container, TEM, SEM Figure 1 As shown in the figure, the modified nano concave spheres are uniform and dispersed in size, with a diameter of about 300-400nm, a shell thickness of about 30nm, and an opening diameter of 150-200nm, similar to a bowl shape, with a uniform opening.

[0060] The BET test results show that the specific surface area of ​​the modified nano concave sphere container prepared in this embodiment is 1500-2200 m 2 / g.

[0061] Multiple EDS results show that the modified nano concave sphere container prepared in this example contains 5% to 15% thiol groups.

[0062] Example 2

[0063] Raw materials: 0.1 mg / mL of modified nano concave sphere container prepared in Example 1, Cd 2+ Cr 6+ The pollutant concentration was 20 mg / L (separate experiments).

[0064] The application method of the modified nano concave ball container for adsorbing heavy metal ions comprises the following steps:

[0065] 1) Add 20mg / L Cd 2+ Cr 6+ 0.1 mg / mL of modified nanoconcave spheres was added to the aqueous solution of pollutants (reaction volume 10 mL);

[0066] 2) adjusting the solution pH to 2-6;

[0067] 3) stirring for 2 hours;

[0068] 4) Centrifuge and measure the concentration of the supernatant;

[0069] like Figure 2 As shown, under different initial pH conditions, Cd 2+ Cr 6+ The removal amount of micropollutants varies with pH. 6+ The adsorption amount decreased with the increase of pH. When pH was 2, the adsorption amount exceeded 380 mg / g. 2+ The adsorption amount reaches a maximum value of nearly 140 mg / g at pH 4.

[0070] like Figure 3 The XPS test results show that Cr 6+ During the adsorption process, it was converted into Cr 3+ , while in Cd 2+ During the adsorption process, -SH was oxidized to -SO4, indicating that the modified nano-concave sphere container also underwent redox reaction during adsorption.

[0071] Example 3

[0072] Raw materials: modified nano concave sphere container prepared in Example 1 0.05-0.4 mg / mL, Cd 2+ Cr 6+The pollutant concentrations were 20 mg / L respectively.

[0073] The heavy metal micro-pollutant adsorption method based on the modified nano concave sphere container comprises the following steps:

[0074] 1) Add 20mg / L Cd 2+ Cr 6+ 0.05-0.4 mg / mL of modified nano concave sphere container was added to the aqueous solution of pollutants;

[0075] 2) Adjust the pH values ​​to 4 (Cd 2+ ) and 2(Cr 6+ );

[0076] 3) stirring for 2 hours;

[0077] 4) Centrifuge and measure the concentration of the supernatant;

[0078] By changing the dosage of adsorbent, the maximum adsorption capacity of the adsorbent was investigated. Figure 4 It can be found that when the adsorbent dosage is 0.05 mg / mL, Cr 6+ The adsorption capacity of Cd reached 1130 mg / g, and the removal rate was close to 90%. 2+ The optimal dosage is also 0.05 mg / g, the maximum adsorption capacity is about 580 mg / g, and the removal rate is about 65%.

[0079] Example 4

[0080] Raw materials: modified nano concave sphere container 0.1mg / mL, adjusted Cd 2+ Cr 6+ Pollutant concentration.

[0081] The heavy metal micro-pollutant adsorption method based on the modified nano concave sphere container comprises the following steps:

[0082] 1) Cd under different concentration conditions 2+ Cr 6+ 0.1 mg / mL of modified nano concave sphere container was added to the pollutants respectively;

[0083] 2) Adjust the pH value to 4 (Cd 2+ ) and 2(Cr 6+ );

[0084] 3) stirring for 2 hours;

[0085] 4) Centrifuge and measure the concentration of the supernatant;

[0086] By changing the initial concentration of pollutants, the adsorption kinetics were investigated. Figure 5 It can be found that Cd 2+Cr 6+ The adsorption was in accordance with the Langmuir adsorption isotherm, and the linear relationship was over 0.95.

[0087] Example 5

[0088] Raw materials: 0.1 mg / mL of the modified nano concave sphere container in Example 1. The concentration of one pollutant was fixed (20 mg / L), and the concentration of the other pollutant was changed to investigate the competitive adsorption of the two pollutants.

[0089] The heavy metal micro-pollutant adsorption method based on the modified nano concave sphere container comprises the following steps:

[0090] 1) Cd under different concentration conditions 2+ / Cr 6+ ( Figure 6 ),Cr 6+ / Cd 2+ ( Figure 7 ), Cd 2+ / As 3+ ( Figure 8 ) 0.1 mg / mL of modified nano concave sphere container was added to the mixed pollutants respectively;

[0091] 2) Change Cr 6+ (10-100mg / L)( Figure 6 ), Cd 2+ (5-40mg / L)( Figure 7 ), Cd 2+ (5-40mg / L)( Figure 8 ), respectively mixed Cd 2+ (20mg / L)( Figure 6 ),Cr 6+ (20mg / L)( Figure 7 ),As 3+ (20mg / L)( Figure 8 );

[0092] 3) Adjust the pH value to 4 ( Figure 6 ) and 2( Figure 7 , Figure 8 );

[0093] 4) stirring for 2h;

[0094] 5) Centrifuge and measure the concentration of the supernatant;

[0095] By changing the initial concentration of one pollutant in the mixed pollutants, competitive adsorption was investigated. Figure 6 The results showed that with the increase of Cr 6+ The initial concentration increased, Cd 2+The adsorption amount showed an upward trend, but the overall change was not significant; Figure 7 It shows that changing Cd 2+ The initial concentration, Cr 6+ The adsorption amount of Cr 6+ The total adsorption amount is decreased; Figure 8 As 3+ The adsorption amount of Cd 2+ The initial concentration of As 3+ and Cd 2+ Compete for adsorption on the same site.

[0096] Example 6

[0097] Raw materials: modified nano concave sphere container prepared in Example 1 0.1 mg / mL, As 3+ , Pb 2+ The pollutant concentrations were 20 mg / L respectively.

[0098] A method for adsorbing heavy metal micropollutants based on a modified nano concave sphere container comprises the following steps:

[0099] 1) Add 20 mg / L As 3+ , Pb 2+ 0.1 mg / mL of modified nano concave sphere container was added to the aqueous solution of pollutants;

[0100] 2) Adjust the pH to 2-12 respectively;

[0101] 3) stirring for 2 hours;

[0102] 4) Centrifuge and measure the concentration of the supernatant;

[0103] like Fig. 9 As shown, under different initial pH conditions, As 3+ , Pb 2+ The removal amount of micropollutants varies with pH. The pH value has a great influence on As 3+ The adsorption amount and adsorption rate did not change much, and the adsorption amount was close to 70 mg / g; while Pb 2+ The adsorption amount and adsorption rate first increased and then decreased with the pH value, reaching a maximum value of nearly 40 mg / g when the pH value was 4.

[0104] Example 7

[0105] Raw materials: 0.05-0.4 mg / mL of modified nano concave sphere container prepared in Example 1, As 3+ , Pb 2+ The dye concentration was 20 mg / L.

[0106] The heavy metal micro-pollutant adsorption method based on the modified nano concave sphere container comprises the following steps:

[0107] 1) Add 20 mg / L As 3+ , Pb 2+ 0.05-0.4 mg / mL of modified nano concave spheres were added to the pollutants;

[0108] 2) Adjust the pH value to 7 (As 3+ ) and 4(Pb 2+ );

[0109] 3) stirring for 2 hours;

[0110] 4) Centrifuge and measure the concentration of the supernatant;

[0111] like Fig.10 As shown in the figure, by changing the dosage of the adsorbent, the maximum adsorption capacity of the adsorbent is investigated. It can be found from the figure that when the dosage of the adsorbent is 0.05 mg / mL, As 3+ The adsorption capacity of Pb is close to 150 mg / g, and the removal rate is about 50%. 2+ The maximum adsorption capacity is about 45 mg / g.

[0112] Example 8

[0113] Raw materials: 0.1 mg / mL of modified nano concave sphere container prepared in Example 1, adjusted As 3+ , Pb 2+ Pollutant concentration.

[0114] The heavy metal micro-pollutant adsorption method based on the modified nano concave sphere container comprises the following steps:

[0115] 1) Towards As under different concentration conditions 3+ , Pb 2+ 0.1 mg / mL of modified nano concave sphere container was added to the pollutants respectively;

[0116] 2) Adjust the pH value to 7 (As 3+ ) and 4(Pb 2+ );

[0117] 3) stirring for 2 hours;

[0118] 4) Centrifuge and measure the concentration of the supernatant;

[0119] By changing the initial concentration of pollutants, the adsorption kinetics were investigated. Fig.11 It can be found that As 3+ , Pb 2+ The adsorption was in accordance with the Langmuir adsorption isotherm, and the linear relationship was over 0.95.

[0120] Example 9

[0121] Raw materials: 0.1 mg / mL of the modified nano concave sphere container prepared in Example 1. The concentration of one pollutant was fixed, and the concentration of another pollutant was changed to investigate the competitive adsorption of the two pollutants.

[0122] The heavy metal micro-pollutant adsorption method based on the modified nano concave sphere container comprises the following steps:

[0123] 1) Change As 3+ The initial concentration of pollutants was 0-20 mg / L, and 20 mg / L of Pb was added to each 2+ ( Fig.12 ),Cr 6+ ( Fig.13 );

[0124] 2) adding 0.1 mg / mL of modified nano concave sphere container to the mixed solution;

[0125] 3) Adjust the pH value to 7;

[0126] 4) stirring for 2h;

[0127] 5) Centrifuge and measure the concentration of the supernatant;

[0128] By changing the initial concentration of one pollutant in the mixed pollutants, competitive adsorption was investigated. Fig.12 , 13 The results showed that with the increase of As 3+ The initial concentration increased, Pb 2+ The adsorption amount of Cr 6+ The adsorption amount of Cr 6+ When present, As 3+ The absolute adsorption amount of Cr 6+ Not with As 3+ compete.

[0129] The above content is a schematic description of the present invention and its implementation methods, which is not restrictive. What is shown in the embodiment is only one of the implementation methods of the present invention, and the actual implementation method is not limited thereto. Therefore, if a person of ordinary skill in the art is inspired by it and designs implementation methods and embodiments similar to the technical solution without creative design without departing from the purpose of the invention, they should all fall within the scope of protection of the present invention.

Claims

1. The application of modified nano concave sphere container in adsorbing heavy metal micro-pollutants is characterized by: The preparation method of the modified nano concave sphere container comprises the following steps: 1) dissolving 3-aminophenol in water, adding formaldehyde and ammonia water to the solution, stirring and causing a polymerization reaction; the mass volume ratio of 3-aminophenol to formaldehyde is (1-2) mg:1 mL; 2) Add acetone to the system after the reaction in step 1), stir, and continue the reaction; the volume ratio of water in step 1) to acetone in step 2) is (1-2):1; 3) Centrifuge to obtain a hollow concave sphere; 4) The hollow concave spheres of step 3) are modified with thiol groups by using 4-aminothiophenol to obtain a modified nano concave sphere container; the modified nano concave sphere container has a bowl-shaped collapsed nano concave sphere with a particle size of 300-500 nm; the weight ratio of thiol groups loaded on the surface of the modified nano concave sphere container is 5%-15%; the specific surface area of ​​the modified nano concave sphere container is 1500-2200 m 2 / g; The heavy metal micropollutants include heavy metal ions Cr 6+ ; Heavy metal ions Cr in heavy metal micropollutants 6+ The concentration is 10~100 mg / L.

2. The use according to claim 1, characterized in that The polymerization reaction time in step 1) is 20 to 60 min.

3. The use according to claim 1, characterized in that The concentration of the modified nano concave sphere container is 0.05-0.4 mg / mL.

4. The use according to claim 1, characterized in that The pH value suitable for the modified nano concave sphere container to adsorb heavy metal micro-pollutants is 1-9.