A silk fibroin liquid crystal suspension and its preparation method and application
Through the combination of heat treatment and low-concentration alkaline reagents, the problems of crystallization zone destruction and the use of harmful reagents during the peeling process of silk protein fibers were solved, and silk protein nanofibers with high crystallinity were obtained, realizing their wide application in liquid crystals. and green preparation.
Patent Information
- Application Number
- CN202310070514.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-20
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-01-20
AI Technical Summary
The existing technology easily destroys the crystalline region of the fiber when stripping silk protein fibers, uses harmful reagents, and has low nanofiber yield and poor stability, which limits its application in liquid crystals.
Heat treatment and low-concentration alkaline reagents are used to destroy the hydrogen bonds between fibers, and are further hydrolyzed to retain the structure of the crystalline region. Silk protein nanofibers with high crystallinity are obtained through ultrasonic dispersion to achieve self-assembly and liquid crystal properties.
Silk protein nanofibers with a complete crystalline region structure have been obtained, realizing their wide application in many fields, including biomedicine and optoelectronics. The preparation process is green, has high stability and high yield.
Smart Images

Figure CN115960467B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of new liquid crystal materials, and in particular to a silk fibroin liquid crystal suspension and a preparation method and application thereof. Background Art
[0002] Liquid crystal is considered to be the fourth state of matter, which can show properties between crystals and isotropic liquids. At present, liquid crystals are mainly based on biomass materials, among which proteins have good biocompatibility and degradation products are small amino acid molecules that are easily absorbed by the human body. They have been widely explored in recent years. Amyloid protein is a new type of liquid crystal material. However, the low yield and high price of amyloid protein liquid crystals limit its development.
[0003] Silk protein fibers are used in textiles, tissue engineering, biomedicine, food, and cosmetics due to their high tensile strength, stiffness, and toughness. Due to the presence of the crystalline region, silk fibers have good orientation and mechanical properties. If the crystalline region is successfully used as a basic building block to construct new silk protein materials with different forms and functions, this will promote the further development of silk protein materials. Therefore, retaining the crystalline region of silk fibers to the greatest extent and stripping them into nano units has become a hot topic and difficulty in current research.
[0004] At present, silk fibers have been stripped into nanofibers by various methods, such as Appl. Phys. Lett. 2007, 90 (7), 073112073112. The high-intensity ultrasound method and the solvent dissolution method, including formic acid / lithium bromide, formic acid / calcium chloride, low eutectic solvent, hexafluoroisopropanol, sulfuric acid, etc., see Biomacromolecules, 2016, 17 (9), 3000-3006; ACS AppLMater. Interfaces 2015, 7 (5), 3352-3361; ACS SustainableChem.Eng.2020, 8(11), 4499-4510; Adv.Mater2016, 28(35), 7783-7791.J.Mater.Chem.B2019, 7(9), 1450-1459.), or alkaline reagents combined with freeze-thaw methods, such as ACSNano 2018, 12(12), 11860-11870, etc.
[0005] Chinese invention patent CN114163684A discloses a method for directly extracting silk nanofibers from discarded silk cocoons and recovering hydrolyzed silk protein and extract. The method adopts a scheme of how to hydrolyze silk fibers through reagents, but no further in-depth research is conducted on the pretreatment of silk. In addition, the stripping conditions adopted are very harsh, and the solution destroys the crystalline region of silk fibroin. In addition, there is also a method of obtaining nanofibers by a bottom-up method (inducing silk protein solution to aggregate into nanofibers), but since the nanofibers are aggregated from disordered molecular chains, the obtained silk fibroin nanofibers have low crystallinity and do not have birefringence, such as a silkworm silk fibroin nanofiber and a preparation method thereof disclosed in Chinese invention patent CN106757447A.
[0006] Chinese invention patent CN 113818096 A discloses a method for preparing and using silk protein nanofibers, wherein silk is added to an alkaline solution to obtain a mixed solution, and the water-insoluble matter in the solid suspension is separated by freeze-thaw or heating and stirring, and the silk protein nanofibers are obtained by mechanical treatment. Although the invention effectively regulates the degree of damage to the structure of the silk protein fiber by alkali by controlling the hydrolysis conditions, the crystallization area is retained to a certain extent, so that the nanofiber dispersion has birefringence under a polarizing microscope. However, according to Chinese invention patent CN 106046133 A, during the repeated freeze-thaw process of silk fibers under alkaline conditions, the repeated growth of ice crystals will destroy the hydrogen bonds in the silk protein molecules and open the crystallization area, and it is easy to obtain silk protein nanoribbons. Therefore, the nanofiber dispersion obtained by Chinese invention patent CN 113818096 A is stably dispersed after 90 days, and does not show phase separation phenomenon and self-assembly process.
[0007] In summary, the existing disclosed technologies have the following technical problems: (1) The stripping or hydrolysis method has a high degree of hydrolysis on the fiber, which is easy to destroy the crystalline region of the fiber, resulting in an incomplete crystalline region, thereby limiting its application in liquid crystals; (2) The stripping process uses reagents such as formic acid, hexafluoroisopropanol and sulfuric acid that are harmful to the human body and the environment, which cannot be mass-produced and green; (3) The yield of the nanofibers obtained by stripping is low and the stability is poor. Summary of the invention
[0008] In view of this, in order to solve the above problems, the present invention provides a silk fibroin liquid crystal suspension and a preparation method and application thereof, adopting mild methods such as heat treatment to first destroy the weaker hydrogen bonds between the fibers, and then further hydrolyze the fibers with a lower concentration of alkaline reagent to obtain silk fibroin nanofibers with higher crystallinity, further expanding the application of silk fibroin liquid crystals in multiple fields.
[0009] In order to achieve the above-mentioned purpose, the present invention provides a silk fibroin nanofiber liquid crystal suspension, which is formed by mixing nanofibers and water; the silk fibroin nanofibers have a complete crystalline region structure; the silk fibroin nanofibers have the ability to spontaneously form nematic liquid crystals and exhibit the characteristics of lyotropic liquid crystals, and have self-assembly behavior.
[0010] Preferably, the content of the silk fibroin nanofibers is 0.01 to 20 wt %, the diameter is 10 to 800 nm, and the length is 50 nm to 200 μm; the self-assembly behavior of the silk fibroin nanofibers is captured by a chemical cross-linking method; the conditions for spontaneous formation of nematic liquid crystals are a temperature of 2 to 80° C. and a humidity of 20 to 99%; and / or, the liquid crystal phase of the crystalline region structure exhibits a birefringence phenomenon, a schlieren texture, and presents rainbow light under orthogonal polarized light.
[0011] Preferably, the surface of the silk fibroin nanofiber has a negative charge as a whole; the arrangement direction of the silk fibroin nanofiber is consistent, and has a uniform orientation regulation effect under the action of a magnetic field and / or an electric field; and / or the protein structure of the silk fibroin nanofiber is a β-folded structure;
[0012] Preferably, the silk fibroin nanofiber liquid crystal suspension is prepared by a method of silk fiber heat treatment-alkaline hydrolysis-ion removal-ultrasonic dispersion; and / or, the silk fibroin nanofiber liquid crystal suspension is diluted with dehydrated water and sealed and refrigerated to produce phase separation; the concentration of the silk fibroin nanofiber liquid crystal suspension that undergoes phase separation is 2-5%.
[0013] To achieve another object, the present invention also provides another technical solution, the preparation method of the silk fibroin nanofiber liquid crystal suspension, the specific steps include:
[0014] S1. Silk fiber heat treatment: The silk fiber is subjected to water bath heat treatment;
[0015] S2. Alkaline hydrolysis: placing the silk fibers treated in S1 in an alkaline solution and stirring until they are dispersed into micro-nanofibers;
[0016] S3. Ion removal: The micro-nanofibers dispersed in S2 were collected by centrifugation and dialyzed with pure water to remove ions;
[0017] S4. Ultrasonic dispersion: The micro-nanofibers after dialysis in S3 are ultrasonically dispersed to obtain a silk fibroin liquid crystal suspension.
[0018] Preferably, in S1, the alkaline solution in the water bath heat treatment is a weak alkaline solution, including one or more combinations of sodium carbonate, sodium phosphate or sodium bicarbonate solution; the biological enzyme is one or more combinations of papain, trypsin, alkaline protease, neutral protease or flavor protease; the silk fiber source is spiders and silkworms; spiders include any one or more combinations of hunting spiders, web-building spiders or cave spiders; silkworms include any one or more combinations of mulberry silkworms, tussah silkworms, wild silkworms or transgenic silkworms.
[0019] Preferably, in S2, the alkaline hydrolysis includes placing the silk fibers in an alkaline solution and stirring until the silk fibers are dispersed into micro-nano fibers, the stirring method includes magnetic stirring, homogenous stirring or turbine stirring, the stirring temperature is 2 to 100°C, the stirring time is 2 to 720 hours, the mass volume ratio concentration of the alkaline solution is 0.5 to 10 g / L, and the bath ratio of the silk fibers to the alkaline solution is 0.1 to 100 g / 1L.
[0020] Preferably, the alkaline solution is any one or more of potassium hydroxide, sodium hydroxide, calcium hydroxide or lithium hydroxide solution.
[0021] Preferably, in S3, the centrifugal collection includes subjecting the nanofibers to a process of centrifugation-pure water suspension-centrifugation, repeating the pure water suspension and centrifugation 3-5 times, and then sealing them in a dialysis bag to remove ions by pure water dialysis; the rotation speed of the centrifugal collection is 5000-20000 rpm, and the centrifugation time is 5-20 min; the dialysis time is 1-5 days, and the molecular weight cutoff of the dialysis bag is 3.5-100 KDa.
[0022] In S4, the power of the ultrasonic dispersion is 50 to 1000 W, and the time of the ultrasonic dispersion is 5 to 800 min.
[0023] In the silk fibroin nanofiber liquid crystal suspension provided by the above technical solution or the silk fibroin nanofiber liquid crystal suspension prepared by the above method, a polymerization monomer, an initiator and a cross-linking agent are added, and after stirring and refrigeration, the silk fibroin nanofiber suspension is induced to react to form a polyacrylamide / silk composite hydrogel under ultraviolet irradiation conditions. That is, the self-assembly behavior of silk fibroin nanofibers can be captured by chemical cross-linking to form a silk fibroin liquid crystal hydrogel; the conditions for spontaneous formation of nematic liquid crystals are temperature 2-80°C, humidity 20-99%, preferably, temperature 2-30°C, humidity 50-95%.
[0024] Furthermore, a polymerizable monomer, an initiator and a cross-linking agent are added to the silk fibroin nanofiber suspension provided by the above technical solution, and after stirring and refrigerating, the silk fibroin nanofiber suspension is induced to react under ultraviolet irradiation to generate the polyacrylamide / silk composite hydrogel. The polyacrylamide / silk composite hydrogel has a phase separation phenomenon, and the upper and lower layers have different microscopic morphologies, the upper layer is isotropic, and the lower layer is anisotropic, and the arrangement direction of the nanofibers in the long-range range is parallel to the phase separation interface.
[0025] Furthermore, the silk fibroin nanofiber liquid crystal suspension provided by the above technical solution or the silk fibroin nanofiber liquid crystal suspension prepared by the above method is air-dried at room temperature to form a film to obtain a silk fibroin liquid crystal film; the silk fibroin liquid crystal film is an anisotropic silk film; it has rainbow colors under orthogonal polarized light conditions; the arrangement of the silk fibroin nanofibers has a spiral structure with chiral structural characteristics.
[0026] Furthermore, the silk fibroin nanofiber liquid crystal suspension provided by the above technical solution or the silk fibroin nanofiber liquid crystal suspension prepared by the above method is placed in hydrochloric acid vapor and sealed for storage to obtain a silk fibroin liquid crystal hydrogel.
[0027] The silk fibroin liquid crystal hydrogel is placed in ethanol for solvent exchange, and then freeze-dried to obtain the silk fibroin liquid crystal aerogel.
[0028] The silk fibroin nanofibers prepared by the above preparation method have the characteristics of uniform and controllable size. Silk fibroin nanofibers with different size requirements can be prepared by selecting different cellulose-containing materials.
[0029] The silk fibroin nanofiber liquid crystal suspension prepared by the technical solution of the present invention has a negative charge on the surface of the nanofiber as a whole, and has a uniform orientation regulation effect under the action of a magnetic field and / or an electric field; at the same time, the nanofiber protein has a complete crystalline region, and the self-assembly behavior of the silk fibroin nanofiber can be captured by a chemical cross-linking method to form a polyacrylamide / silk composite hydrogel, that is, it can spontaneously form a nematic liquid crystal and exhibit the characteristics of a lyotropic liquid crystal, and has a self-assembly behavior.
[0030] Beneficial technical effects obtained by the present invention:
[0031] 1. The technical solution of the present invention is used to prepare a silk fibroin nanofiber suspension, which combines heat treatment with low alkali concentration. Through the early heat treatment, some intermolecular forces between silk fibers are opened, and the concentration of the later alkali treatment is effectively reduced, thereby retaining the crystalline region structure of the silk fibroin. The nanofibers obtained by peeling after water bath heat treatment have a relatively complete crystalline region structure, and can spontaneously form nematic liquid crystals in aqueous solution. After dilution, driven by entropy, the silk fibroin nanofiber suspension undergoes phase separation.
[0032] 2. The nanofiber surface obtained by alkaline solution stripping of the silk fibroin nanofiber suspension prepared by the technical solution of the present invention has abundant carboxyl groups, so that the nanofiber suspension is negatively charged as a whole. The repulsive effect of the negative charges between the nanofibers is beneficial to improving the stability of the fiber dispersion.
[0033] 3. By adopting the technical solution of the present invention and selecting a lower concentration of alkaline reagent, the obtained silk fibroin nanofibers have a higher yield; and no toxic reagents and volatile drugs are used in the entire preparation process, which has potential advantages in green preparation, processing and mass production.
[0034] 4. The silk fibroin nanofibers obtained by the technical solution of the present invention can be used to prepare polyacrylamide / silk composite hydrogel. After drying and gold spraying, the hydrogel has a clear interface, and the upper and lower layers have different microscopic morphologies. The upper layer is isotropic and the lower layer is anisotropic. The arrangement direction of the nanofibers is parallel to the phase separation interface and can be applied in the field of biomedicine.
[0035] 5. The hydrogel obtained by the technical solution of the present invention is subjected to solvent replacement and then freeze-dried to obtain silk fibroin liquid crystal aerogel, which has rainbow color under a polarizing microscope and can be applied in the field of optoelectronics.
[0036] 6. After the silk fibroin nanofiber suspension is prepared by the technical solution of the present invention and air-dried to form a film, the arrangement of the nanofibers in the obtained film has a certain spiral structure, indicating that the silk fibroin liquid crystal film has a certain chiral structure. Its birefringence phenomenon is observed under orthogonal polarizers, and the film has a significant rainbow color, which can be applied in the field of optoelectronics.
[0037] 7. The silk fibroin nanofiber suspension prepared by the technical solution of the present invention has a simple preparation process and broad application prospects. It can be widely used in biology, medicine, composite materials, optics and other fields and is easy to promote and apply. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is an AFM morphology image of the silk fibroin nanofibers in the silk fibroin nanofiber liquid crystal suspension prepared in Example 1 of the present invention.
[0039] Figure 2a This is a microscope photograph of the silk fibroin nanofiber liquid crystal suspension prepared in Example 1 of the present invention under orthogonal polarization conditions.
[0040] Figure 2b This is a microscope photograph of the silk fibroin nanofiber suspension prepared in Example 1 of the present invention after the polarizer is rotated 45°.
[0041] Figure 3 This is the circular dichroism (CD) spectrum of the silk fibroin nanofiber suspension prepared in Example 1 of the present invention.
[0042] Figure 4 This is a polarizing microscope photograph of the silk fibroin nanofiber suspension prepared in Example 1 of the present invention under orthogonal polarized light.
[0043] Figure 5 This is a photograph of the phase separation test results of the silk fibroin nanofiber suspension prepared in Example 5 of the present invention at 168 hours.
[0044] Figure 6 This is an electronic photograph of the polyacrylamide / silk composite hydrogel prepared in Example 8 of the present invention.
[0045] Figure 7 The interface morphology of the phase separation of the polyacrylamide / silk composite hydrogel prepared in Example 8 of the present invention was observed under a scanning electron microscope.
[0046] Figure 8 This is a SEM microscopic morphology of the phase separation of the polyacrylamide / silk composite hydrogel prepared in Example 8 of the present invention.
[0047] Fig. 9 This is the infrared spectrum of the silk fibroin liquid crystal film prepared in Example 9 of the present invention and the silk fiber before hydrolysis.
[0048] Fig.10 XRD patterns of the silk fibroin liquid crystal film prepared in Example 9 of the present invention and the silk fiber before hydrolysis.
[0049] Fig.11 This is a comparison chart of polarized photos of the silk fibroin liquid crystal film prepared in Example 9 of the present invention and the silk fibroin film prepared in Control Example 1.
[0050] Fig.12 This is a SEM microscopic morphology image of the silk fibroin liquid crystal film prepared in Example 9 of the present invention.
[0051] Fig.13 This is a SEM microscopic morphology image of the silk fibroin film prepared in Control Example 1 of the present invention.
[0052] Fig.14a This is an electronic photograph of the silk fibroin liquid crystal aerogel prepared in Example 10 of the present invention.
[0053] Fig.14b This is a SEM microscopic morphology image of the silk fibroin liquid crystal aerogel prepared in Example 10 of the present invention.
[0054] Fig.14c This is a polarizing microscope image of the silk fibroin liquid crystal aerogel prepared in Example 10 of the present invention.
[0055] Fig.15a and Fig.15b They are polarized photographs of the silk fibroin liquid crystal suspension prepared in Example 10 of the present invention under the action of different electric field forces.
[0056] Fig.16 This is a polarizing microscope image of the silk fibroin solution of Control Example 1 of the present invention taken with orthogonal polarized light. DETAILED DESCRIPTION
[0057] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application will be clearly and completely described below in combination with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments.
[0058] The present invention provides a silk fibroin nanofiber liquid crystal suspension, which is formed by mixing silk fibroin nanofibers and water; the silk fibroin nanofibers have a complete crystalline region structure; the silk fibroin nanofibers have the characteristics of spontaneously forming nematic liquid crystals and showing lyotropic liquid crystals, and have self-assembly behavior. The self-assembly behavior can be captured by a chemical cross-linking method, and the obtained polymer / silk hydrogel has the characteristics of phase separation.
[0059] At the same time, the arrangement of nanofibers in the silk fibroin nanofiber film prepared by using the silk fibroin nanofiber suspension has a certain spiral structure, and the silk fibroin nanofiber hydrogel and / or silk fibroin nanofiber aerogel can be observed as rainbow color under polarized light.
[0060] The technical solution of the present invention is further described in detail below through specific embodiments.
[0061] Example 1
[0062] This embodiment provides a method for preparing a liquid crystal suspension of silk fibroin nanofibers, and selects silk from Bombyx mori as the raw material of silk fibroin. Bombyx mori silk is composed of two parallel silk fibroin fibers and an outer layer of sericin. The sericin encapsulates the two fibers, which is more conducive to the molding of the fibers and acts as an adhesive. In order to obtain silk fibroin, the outer layer of sericin needs to be removed. The outer layer of sericin is a water-soluble protein that is easily soluble in hot water, enzymes and weak alkaline solutions.
[0063] This embodiment provides a method for preparing a silk fibroin nanofiber liquid crystal suspension, and the specific steps include:
[0064] (1) Prepare 1L of sodium carbonate solution with a concentration of 0.05% (mass to volume), immerse silk in the solution, maintain the bath ratio of silk to sodium carbonate solution at 0.5g / 1L, 2g / 1L, 5g / 1L, 10g / 1L, 15g / 1L, 20g / 1L and 50g / 1L, heat and boil respectively for 30 minutes to carry out degumming treatment, the purpose of the treatment method is not only to remove sericin, but also to destroy the weaker interaction between fibers.
[0065] The degummed silk was washed in pure water for 3-5 times, dried in a 45-degree oven to constant weight, and the weight after drying was recorded to calculate the degumming loss rate of the silk. The results are shown in Table 1. It was calculated that the loss rate of the silk mass after treatment was 15%-42.5%.
[0066] Table 1 Degumming loss rate of silk treated under different bath ratio conditions
[0067] Bath ratio 0.5g / 1L 2g / 1L 5g / 1L 10g / 1L 15g / lL 20g / lL 50g / 1L Degumming rate 42.5% 26.3% 25.1% 24.7% 22.6% 21.3% 15%
[0068] In this embodiment, Bombyx mori silk is selected as the raw material of silk fibroin, and its sericin accounts for about 25% of the whole silk. Therefore, it can be seen from the results in Table 1 that the subsequent steps are preferably carried out under the heat treatment conditions of a bath ratio of 10 g / L and a degumming rate of 24.7%. When other silks are selected as the raw material of silk fibroin, the bath ratio can be selected according to the sericin content of the silk.
[0069] (2) preparing a potassium hydroxide solution with a concentration of 5 g / L, adding the fibers obtained by heat treatment in step (1) at a bath ratio of 10 g:1 L of silk to alkaline solution to the alkaline solution, and stirring by magnetic force until the fibers are dispersed into micro-nanofibers, the stirring temperature is 25° C., and the stirring time is 10 days.
[0070] (3) The silk micro-nano fibers obtained in step (2) are centrifuged with potassium hydroxide solution at 12,000 rpm for 10 min. The nanofibers obtained by stripping have a diameter of about 200 nm to 600 nm and a length of about 1 μm to 20 μm.
[0071] (4) After centrifugation, the precipitate was collected and transferred to a dialysis bag with a molecular weight cutoff of 3500 Da and dialyzed in deionized water for 5 days.
[0072] (5) The dialyzed fibers were dispersed by ultrasonication (Fisherbrand Ultrasonic disintegrator, 660 Hz) to obtain a silk fibroin nanofiber suspension with good dispersibility. The ultrasonic dispersion power was 500 W and the ultrasonic dispersion time was 20 min.
[0073] A nanofiber suspension of known weight (referred to as w1) is placed in a 60°C oven and dried to constant weight, and then weighed as w2. The ratio of w2 to w1 is multiplied by 100% to obtain the concentration of the nanofibers. The concentration of the silk fibroin nanofiber suspension in this example is about 4.5%.
[0074] Morphology observation: The silk fibroin nanofiber suspension prepared in the above steps was diluted to a concentration of 0.5%, and the morphology was observed by AFM. Figure 1 , is an AFM (instrument: Bruker AXS D8) morphology image of the silk fibroin nanofibers of this example. The obtained nanofibers have a diameter of about 40 to 60 nm and a length of 100 to 600 nm.
[0075] Polarized light observation: Take a small amount of 3% nanofiber suspension and observe the liquid crystal phase of the nanofibers under a polarizing microscope (BM2100POL). Figure 2a and Figure 2b ,in, Figure 2a This is a microscope photo taken under orthogonal polarization conditions. Figure 2b This is a microscope photo after the polarizer was rotated 45°. Through observation, it was found that the nanofibers obtained by the present invention had obvious birefringence and clear schlieren texture. The liquid crystal phase had different colors at different angles, indicating that it had direction dependence and anisotropy, and had the basic characteristics of liquid crystal.
[0076] See also Figure 4 , is a polarizing microscope image of a silk fibroin nanofiber suspension under orthogonal polarized light, showing rainbow light under orthogonal polarized light.
[0077] Potential measurement of nanofiber suspension: The nanofiber suspension was diluted to 0.01% with deionized water and transferred to a potential measurement cell. The potential of the nanofiber suspension was measured in a Malvern potentiostat (Nano ZS ZEN3600). The surface of the silk fibroin nanofibers was negatively charged (about -45 mV) as a whole, which further proved that the surface of the silk fibroin nanofibers contained a large number of carboxyl groups.
[0078] Crystal structure determination: The silk fibroin nanofiber dispersion was diluted to 0.01% and transferred to a 10 mm cuvette. A circular dichroism (CD) spectrometer (Chirascan-plus) was used to collect the CD spectrum of the silk fibroin fiber dispersion. The collected spectrum range was 190-250nm, the spectrum scanning speed was 100nm / min, the resolution was 1nm, and pure water was used as the control group.
[0079] See also Figure 3 , is the circular dichroism (CD) spectrum of the silk fibroin nanofiber suspension. It can be seen from the spectrum that the silk fibroin nanofiber suspension has characteristic peaks near 195.2nm and 219.1nm, indicating that the protein structure in the nanofiber is a β-folded structure, indicating that the silk fibroin nanofiber retains the β-folded structure of silk.
[0080] Example 2
[0081] This embodiment provides a method for preparing a silk fibroin nanofiber suspension, wherein sodium hydroxide is used to strip silk fibers, and the specific steps include:
[0082] (1) Prepare 100 mL of papain solution with concentrations of 0.5%, 1% and 2%, respectively, place in a water bath and heat to 85-90°C, then immerse 1 g of silk in the solution for 1 hour, take out and wash with deionized water 5 times, place in a 45°C oven and dry to constant weight, and finally record the weight after drying.
[0083] It was calculated that the mass loss rates of silk after treatment with papain solution at concentrations of 0.5%, 1% and 2% were 13.5%, 19.9% and 25.8% respectively. The residual sericin was evaluated by picric acid-carmine reagent. The results showed that after the silk was treated with 0.5% protease solution, sericin remained on the surface, 1% had almost no sericin residue, and 2% had no sericin residue.
[0084] In order to preserve the silk structure as much as possible, the subsequent experiments selected silk fibers treated with a papain solution concentration of 1%.
[0085] (2) Prepare a sodium hydroxide solution with a concentration of 3 g / L (mass volume ratio concentration), add the silk fibers degummed with 1% protease solution in (1) into the alkaline solution, the bath ratio of silk to alkaline solution is 40 g:1 L, and stir uniformly until the fibers are dispersed into micro-nano fibers, the stirring temperature is 45° C., and the stirring time is 3 days. Then, centrifuge the mixture of silk fibers and alkali at 11000 rpm for 10 min. After the centrifugation, collect the precipitate, transfer it to a dialysis bag with a molecular weight cutoff of 14000 Da, and dialyze it in deionized water for 5 days.
[0086] (3) The dialyzed fibers were passed through a cell crusher to obtain a nanofiber suspension with good dispersibility. The ultrasonic dispersion power was 200 W and the ultrasonic dispersion time was 50 min. Fibers with a diameter of about 20-80 nm and a length of 100-900 nm were obtained.
[0087] Example 3
[0088] This embodiment provides a method for preparing a silk fibroin nanofiber suspension, wherein sodium bicarbonate is used to strip silk fibers, and the specific steps include:
[0089] (1) Weigh 5g of silk and put it into 100mL of deionized water. Treat it with high temperature and high pressure for 30min. The treatment temperature is 120℃ and the pressure is 0.1MPa. After the treatment, the silk fiber is washed with deionized water for 5 times and placed in a 45℃ oven to dry to constant weight. Finally, the weight after drying is recorded. After calculation, the loss rate of silk mass after treatment is 18.7%.
[0090] (2) Prepare a sodium bicarbonate solution with a concentration of 0.8% (mass to volume), add the fibers obtained in (1) to the alkaline solution, the bath ratio of silk to alkaline solution is 10g:1L, and stir by vortexing until the fibers are dispersed into micro-nano fibers, the stirring temperature is 80°C, and the stirring time is 6h. Then, centrifuge the mixture of silk fibers and alkali at 11000rpm for 10min. After the centrifugation, collect the precipitate, transfer it to a dialysis bag with a molecular weight cutoff of 100KDa, and dialyze it in deionized water for 5 days.
[0091] (3) The dialyzed fibers were dispersed by ultrasonic treatment to obtain a nanofiber suspension with good dispersibility. The ultrasonic dispersion power was 650 W and the ultrasonic dispersion time was 200 min. Fibers with a diameter of 5 to 40 nm and a length of 60 to 1200 nm were obtained.
[0092] Example 4
[0093] This embodiment provides a method for preparing a silk fibroin nanofiber suspension, wherein potassium hydroxide is used to strip silk fibers, and the specific steps include:
[0094] (1) Prepare 1L sodium carbonate solution with a concentration of 0.05% (mass to volume), immerse silk fibers in the sodium carbonate solution, keep the bath ratio of silk to sodium carbonate solution at 10g / 1L, heat and boil for 60 minutes. Then wash 3 to 5 times in pure water, dry in a 45 degree oven to constant weight, and finally record the weight after drying. After calculation, the mass loss rate of silk after treatment is 35.1%.
[0095] (2) Prepare a potassium hydroxide solution with a concentration of 5 g / L (mass to volume), add the fibers obtained in (1) to the alkaline solution, and the bath ratio of silk to alkaline solution is 5 g:1 L. Stir magnetically until the fibers are dispersed into micro-nano fibers. The stirring temperature is 25°C and the stirring time is 7 days. Then, centrifuge the mixture of silk fibers and alkali at 11,000 rpm for 10 min. After the centrifugation, collect the precipitate and transfer it to a dialysis bag with a molecular weight cutoff of 20,000 Da, and dialyze it in deionized water for 5 days.
[0096] (3) The fibers after dialysis are dispersed by ultrasound to obtain a nanofiber suspension with good dispersibility. The power of the ultrasonic dispersion is 400 W and the time of the ultrasonic dispersion is 30 min. After ultrasound, the yield of the nanofibers is about 43.8%.
[0097] Example 5
[0098] This embodiment is an embodiment of phase separation of silk protein nanofiber suspension.
[0099] The nanofiber suspension prepared in Example 1 was diluted with deionized water to a suspension with a mass percentage concentration of 3.5%, sealed and placed in a refrigerator at 4 degrees with a humidity of about 75%. At set time points (12h, 24h, 36h, 48h, 96h, 168h), the phase separation process of the nanofiber suspension was observed by taking photos at 168h. Figure 5 .
[0100] Depend on Figure 5 It can be seen that driven by entropy, the nanofiber suspension gradually separates into two phases.
[0101] Example 6
[0102] The difference between this embodiment and embodiment 5 is that the nanofiber suspension with a diluted concentration of 2% is left to stand at a temperature of 25° C. and a humidity of 50% to observe the phase separation process.
[0103] Example 7
[0104] The difference between this embodiment and embodiment 5 is that the nanofiber suspension with a diluted concentration of 5% is left to stand at a temperature of 4° C. and a humidity of 95% to observe the phase separation process.
[0105] The same phase separation phenomenon as in Example 5 was observed in both Example 6 and Example 7.
[0106] Example 8
[0107] Accurately weighed 0.5 g of monomer acrylamide, 50 mg of cross-linking agent nn′-methylenebis(acrylamide) and 5 mg of 2-hydroxy-4′-(2-hydroxyethoxy)-2-methylacetophenone and 5 mL of 3% silk nanofiber suspension were added to the silk fibroin nanofiber suspension obtained by the preparation method of Example 1, and the mixture was continuously stirred at 500 rpm for 60 minutes. The mixture was placed in a 4°C refrigerator with a humidity of 95%. After one week, phase separation of the silk fibroin nanofiber suspension was observed, and ultraviolet polymerization was carried out for 30 minutes using a 250 W ultraviolet light source to obtain a polyacrylamide / silk composite hydrogel.
[0108] See attached Figure 6 , is an electronic photograph of the polyacrylamide / silk composite hydrogel of this example.
[0109] See attached Figure 7 The composite hydrogel was placed in an oven at 60°C for drying. After gold spraying, the interface morphology at the phase separation point was observed under a scanning electron microscope. It can be observed that the polyacrylamide / silk composite hydrogel has a clear interface.
[0110] See attached Figure 8 The upper and lower layers of the polyacrylamide / silk composite hydrogel have different microscopic morphologies. The upper layer is isotropic and the lower layer is anisotropic. The arrangement direction of the nanofibers in the long range is parallel to the phase separation interface.
[0111] Example 9
[0112] 3.5 mL of the silk fibroin nanofiber suspension prepared in Example 1 was taken and placed in a 35 mm plastic dish, and air-dried at room temperature to form a film, thereby obtaining a silk fibroin nanofiber film, which was an anisotropic film.
[0113] The morphology and structure of the prepared silk protein nanofiber film were characterized.
[0114] 1. Birefringence. The secondary structure of the protein film was determined in the reflection mode using a Fourier transform infrared spectrometer (FTIR, Nicolet 5700) with a measurement range of 400–4000 cm -1 .
[0115] 2. Place the silk protein liquid crystal film in an X-ray diffraction sample cell and use a Bruker AXS D8 Advance to measure the diffraction intensity in the range of 2θ=5-45.
[0116] 3. Scanning electron microscope (S4800, Hitachi) was used to observe the surface and cross-sectional morphology of the films.
[0117] 4. Observe the surface color of the film under a polarized light microscope.
[0118] See also Fig. 9 The infrared spectra of the silk fibroin nanofiber film of this example and the silk fiber before hydrolysis are shown in Figure 1 at 1620 cm -1 and 1510.5cm -1 There are common infrared characteristic peaks at the same time, which shows that the silk fibroin nanofiber film maintains the β-folded structure of silk fiber.
[0119] See also Fig.10 , is the XRD spectrum of the silk fibroin nanofiber film of this embodiment and the silk fiber before hydrolysis, the spectrum can further prove the β-folded structure of the silk fibroin nanofiber film, which further illustrates that the stripping method of this embodiment can retain the β-folded structure of the silk fiber before hydrolysis.
[0120] See also Fig.11 , the silk protein nanofiber film of this embodiment appears rainbow-colored under a polarized light microscope.
[0121] See also Fig.12 The arrangement of nanofibers can be observed in the cross section of the silk fibroin nanofiber film, and the arrangement of nanofibers has a certain spiral structure, indicating that the silk fibroin liquid crystal film has a certain chiral structure.
[0122] Example 10
[0123] The silk liquid crystal suspension prepared in Example 1 was placed in a glass bottle, and then placed in a sealed environment with hydrochloric acid vapor for 3 days to obtain a silk fibroin liquid crystal hydrogel.
[0124] The prepared silk fibroin liquid crystal hydrogel was placed in ethanol for solvent exchange for 2 days, then frozen in a -20°C refrigerator for 24 hours, and dried using a freezing process (instrument model: FD-1A-50) to obtain the silk fibroin liquid crystal aerogel. The freeze-drying conditions were: condensation temperature -40°C, vacuum degree 28Pa.
[0125] Observe the color of silk fibroin liquid crystal aerogel under a polarizing microscope.
[0126] See attached Fig.14a , is an electron photo of silk fibroin nanofiber aerogel; Fig.14b The SEM microstructure of silk fibroin nanofiber aerogel; Fig.14c Polarized microscope image of silk fibroin nanofiber aerogel.
[0127] By attaching Fig.14b and 14c It can be found that silk fibroin liquid crystal aerogel has a significant rainbow color under a microscope.
[0128] Embodiment 11
[0129] This example is an example of an orientation control test of the silk liquid crystal suspension prepared in Example 1.
[0130] The silk liquid crystal suspension prepared in Example 1 was placed in a glass bottle and placed in a magnetic field (magnetic field strength 2T) for magnetic field regulation. A magnetic field force was applied to the nanofibers to regulate the movement direction of the nanofibers, and the nanofibers moved along the direction of the magnetic field force.
[0131] The graphite electrodes were fixed to the opposite sides of the glass square cylinder, and then the silk liquid crystal suspension prepared in Example 1 was placed into the glass square cylinder, and a direct current power supply was connected to perform electric field regulation on the nanofibers.
[0132] Since the surface of the nanofibers carries a negative charge, when a voltage of 5 V / cm and 20 V / cm is applied respectively, the nanofibers will gradually transfer to the positive electrode under the action of the electric field force.
[0133] See attached Fig.15a and 15b , respectively, the orientation of the test nanofibers at voltages of 5V / cm and 20V / cm, and it can be found that both move along the direction of the electric field. Finally, under polarized light, a uniform color can be observed near the positive electrode.
[0134] The above test results show that the arrangement direction of the nanofibers under the action of magnetic field and electric field is consistent, and at a voltage of 5V / cm, they have a more uniform orientation.
[0135] Comparative Example 1
[0136] This comparative example adopts the conventional lithium bromide method in the prior art to prepare the silk fibroin solution, and the specific steps include:
[0137] (1) Prepare 1L sodium carbonate solution with a concentration of 0.2% (mass to volume), immerse silk fibers in the sodium carbonate solution, keep the bath ratio of silk to sodium carbonate solution at 2.5g / 1L, heat and boil for 30 minutes. Then wash 3-5 times in pure water, and dry in a 45 degree oven to constant weight.
[0138] (2) The dried silk was added to 9.3 M lithium bromide with a bath ratio of 1 g of silk to 4 mL. The silk was transferred to an oven at 60 °C for 4 hours and packaged into a dialysis bag with a molecular weight cutoff of 3500 Da. After dialysis for 3 days, the supernatant was collected by centrifugation to obtain a silk fibroin solution with a concentration of about 5-7 w.t%.
[0139] (3) Observe the silk fibroin solution under a polarizing microscope.
[0140] In this comparative example, the method of dissolving the silk fibroin solution using lithium bromide is one of the conventional methods in the art.
[0141] 3.5 mL of the silk fibroin solution was placed in a 35 mm plastic dish and air-dried at room temperature to form a film to obtain a silk fibroin film.
[0142] See also Fig.11 , the silk fibroin solution obtained by the preparation method of this comparative example was observed under a polarizing microscope, and there was no birefringence, it was isotropic, had no chiral structure, and had no color under polarized light. However, the arrangement of nanofibers in the silk fibroin liquid crystal film prepared in Example 9 had a certain helical structure, and rainbow colors could be observed under polarized light.
[0143] See also Fig.13 The cross-sectional morphology of the silk fibroin film is dense, while the arrangement of the nanofibers in the silk fibroin liquid crystal film prepared in Example 9 has a certain spiral structure, and the two have significant differences in structure.
[0144] See also Fig.16 , is a polarization microscope image of the orthogonal polarized light of the silk fibroin solution, there is no color under the orthogonal polarized light, and compared with Example 1, refer to Figure 4 , the silk fibroin suspension prepared in Example 1 exhibited rainbow light.
[0145] Comparative Example 2
[0146] The difference between this comparative example and Example 5 is that the concentration of the nanofiber suspension is 5.5%, and other conditions are the same.
[0147] Comparative Example 3
[0148] The difference between this comparative example and Example 5 is that the concentration of the nanofiber suspension is 1%, and other conditions are the same.
[0149] The phase separation processes of the nanofiber suspensions of Control Example 2 and Control Example 3 were observed respectively, and the phase separation process as in Example 5 did not occur.
[0150] By comparing Examples 5-7 and Comparative Examples 2-3, it can be seen that phase separation occurs within the range of 2-5% concentration of the nanofiber suspension. When the concentration is higher than 5% and lower than 2%, phase separation is difficult to occur. When the concentration is high, the steric hindrance of the nanofibers increases, the local fiber concentration is high, and the birefringence phenomenon is obvious, but it is not easy to produce phase separation; when the concentration is too low, the distance between the nanofibers is far, the nanofibers have a higher free energy, and it is not easy to separate into phases. At this time, the birefringence phenomenon is not obvious. Through the above analysis, it is further proved from the side that the liquid crystal is a lyotropic liquid crystal, that is, it has a liquid crystal phase within a certain concentration.
[0151] In summary, the present invention provides a silk fibroin chiral liquid crystal suspension, a mixed system including but not limited to nanofibers and water, the nanofibers have a controllable aspect ratio; the nanofibers in the suspension can spontaneously form nematic liquid crystals and exhibit the characteristics of lyotropic liquid crystals. The present invention combines heat treatment with low alkali concentration, opens the intermolecular forces between the fibers through early heat treatment, effectively reduces the concentration of later alkali treatment, thereby retaining the crystalline region structure of silk fibroin, and the nanofibers obtained by stripping have a relatively complete crystalline region structure, so nematic liquid crystals can be spontaneously formed in aqueous solution, and the silk fibroin nanofibers have the characteristics of spontaneously forming nematic liquid crystals and exhibiting lyotropic liquid crystals, and have self-assembly behavior. And the present invention captures the self-assembly behavior of silk fibroin nanofibers by chemical crosslinking, and can form anisotropic polymer / silk composite hydrogels. At the same time, the silk fibroin nanofibers provided by the present invention have a phase separation phenomenon that only exists in solute liquid crystal systems.
[0152] Liquid crystals with chiral structures are widely used in fields such as optics, imaging, display, and sensing. The phase separation process is extremely important for the regulation of chirality, and is also a basic characteristic of most solute liquid crystals. For example, vanadium pentoxide, sunset yellow FCF, cellulose nanocrystals, graphene oxide, carbon nanotubes, hydroxyapatite nanorods, chitin nanocrystals, and amyloid nanofibers all have a phase separation process. In general, the silk fibroin liquid crystal phase prepared by the prior art has not shown the above-mentioned phase separation phenomenon. The silk fibroin liquid crystal prepared by the technical solution of the present invention shows the phase separation process, which means that the nanofibers will spontaneously assemble, and after assembly, they often have anisotropy. Anisotropic materials will show different optical properties in the path of light, and can be applied to fields such as gratings and optical anti-counterfeiting materials.
[0153] The silk fibroin nanofibers provided by the present invention have abundant carboxyl groups on the fiber surface, so that the nanofiber suspension has a negative charge as a whole. The repulsive effect of the negative charges between the nanofibers is beneficial to improving the stability of the fiber dispersion. At the same time, the arrangement direction of the nanofibers can be regulated under the action of magnetic and electric fields, and the nanofibers also have high sensitivity to external fields (magnetic and electric fields). This makes the silk protein liquid crystal have potential application value in optical sensing, biomedicine, health food, cosmetics, information encryption and tissue engineering.
[0154] Furthermore, since a relatively low concentration of alkaline reagent is used, the obtained nanofibers have a higher yield; no toxic reagents or volatile chemicals are used in the entire preparation process, which has obvious advantages in green preparation, processing and mass production.
[0155] The above are only preferred embodiments of the present invention, which do not limit the protection scope of the present invention. For those skilled in the art, the present invention may have various modifications and changes. Within the spirit and principle of the present invention, changes, modifications, replacements, integrations and parameter changes to these embodiments by conventional substitutions or capable of achieving the same functions without departing from the principles and spirit of the present invention all fall within the protection scope of the present invention.
Claims
1. A silk fibroin nanofiber liquid crystal suspension, characterized in that: The silk fibroin nanofiber liquid crystal suspension is formed by mixing silk fibroin nanofibers and water; the silk fibroin nanofibers have a complete crystalline region structure; the silk fibroin nanofibers have the characteristics of spontaneously forming nematic liquid crystals and exhibiting lyotropic liquid crystals, and have self-assembly behavior; The silk fibroin nanofiber liquid crystal suspension is prepared by a method of silk fiber heat treatment-alkaline hydrolysis-ion removal-ultrasonic dispersion; The silk fibroin nanofiber liquid crystal suspension is diluted with deionized water to a suspension with a mass percentage concentration of 2-5%, which is the final silk fibroin nanofiber liquid crystal suspension; The final silk fibroin nanofiber liquid crystal suspension was sealed and placed in a refrigerator at 4° C. for 168 hours, and phase separation was observed; The silk fiber heat treatment is to heat treat the silk fiber in a water bath using a weak alkaline solution or a biological enzyme solution; The weak base is a combination of one or more of sodium carbonate, sodium phosphate and sodium bicarbonate; The biological enzyme is a combination of one or more of papain, trypsin, alkaline protease, neutral protease and flavor protease; The mass volume ratio concentration of the weak alkaline solution is 0.05%; the concentration of the biological enzyme solution is 1% or 2%; The alkaline hydrolysis is to place the heat-treated silk fibers in an alkaline solution and stir until they are dispersed into micro-nano fibers; The mass volume ratio concentration of the alkaline solution is 0.3-0.5%; The alkaline solution is any one or more of potassium hydroxide, sodium hydroxide, calcium hydroxide and lithium hydroxide solutions; The surface of the silk fibroin nanofibers carries negative charges as a whole; the arrangement of the silk fibroin nanofibers is consistent in direction within a long range, and has a uniform orientation regulation effect under the action of a magnetic field and / or an electric field.
2. The silk fibroin nanofiber liquid crystal suspension according to claim 1, characterized in that: The diameter of the silk fibroin nanofibers is 10-800 nm, and the length is 50 nm-200 μm; The conditions for spontaneously forming nematic liquid crystal are temperature 2-80° C. and humidity 20-99%; The liquid crystal phase of the crystalline region structure exhibits a birefringence phenomenon, a schlieren texture, and presents rainbow light under orthogonal polarized light; and / or, the self-assembly behavior of the silk protein nanofibers is captured by a chemical cross-linking method.
3. The silk fibroin nanofiber liquid crystal suspension according to claim 1, characterized in that: The protein structure of the silk fibroin nanofiber is a β-folded structure.
4. The method for preparing the silk fibroin nanofiber liquid crystal suspension according to any one of claims 1 to 3, characterized in that: The specific steps include: S1. Heat treatment of silk fibers: heat treatment of silk fibers in a water bath using a weak alkaline solution or a biological enzyme solution; The weak base is a combination of one or more of sodium carbonate, sodium phosphate and sodium bicarbonate; The biological enzyme is any one or more combinations of papain, trypsin, alkaline protease, neutral protease and flavor protease; The mass volume ratio concentration of the weak alkaline solution is 0.05%; the concentration of the biological enzyme solution is 1% or 2%; S2. Alkaline hydrolysis: placing the silk fibers treated in S1 in an alkaline solution and stirring until they are dispersed into micro-nanofibers; The mass volume ratio concentration of the alkaline solution is 0.3-0.5%; The alkaline solution is any one or more of potassium hydroxide, sodium hydroxide, calcium hydroxide and lithium hydroxide solutions; S3. Ion removal: The micro-nanofibers dispersed in S2 were collected by centrifugation and dialyzed with pure water to remove ions; S4. Ultrasonic dispersion: The micro-nanofibers after dialysis in S3 are ultrasonically dispersed to obtain a silk fibroin nanofiber liquid crystal suspension; The silk fibroin nanofiber liquid crystal suspension is diluted with deionized water to a suspension with a mass percentage concentration of 2-5%, which is the final silk fibroin nanofiber liquid crystal suspension.
5. The method for preparing the silk fibroin nanofiber liquid crystal suspension according to claim 4, characterized in that: The silk fibers are derived from spiders and silkworms; spiders include any one or more combinations of hunting spiders, web-building spiders and cave spiders; silkworms include any one or more combinations of mulberry silkworms, tussah silkworms and transgenic silkworms; In S2, the stirring method includes magnetic stirring, homogenous stirring or turbine stirring, the stirring temperature is 2-100° C., the stirring time is 2-720 hours, and the bath ratio of the silk fiber to the alkaline solution is 0.1-100 g / L; In S3, the centrifugal collection includes subjecting the micro-nano fibers to a process of centrifugation-pure water suspension-centrifugation, repeating the pure water suspension and centrifugation 3-5 times, and then sealing the micro-nano fibers in a dialysis bag and dialyzing them with pure water to remove ions; The rotation speed of the centrifugal collection is 5000-20000 rpm, and the centrifugation time is 5-20 min; the dialysis time is 1-5 days, and the molecular weight cutoff of the dialysis bag is 3.5-100KDa; In S4, the power of the ultrasonic dispersion is 50-1000 W, and the time of the ultrasonic dispersion is 5-800 min.
6. A polyacrylamide / silk composite hydrogel, comprising adding acrylamide, an initiator and a cross-linking agent to the silk fibroin nanofiber liquid crystal suspension according to any one of claims 1 to 3, stirring and refrigerating, and then inducing the silk fibroin nanofiber liquid crystal suspension to react under ultraviolet light conditions to generate the polyacrylamide / silk composite hydrogel.
7. A silk fibroin liquid crystal film, comprising: air-drying the silk fibroin nanofiber liquid crystal suspension as described in any one of claims 1 to 3 at room temperature to form a film; the silk fibroin liquid crystal film is an anisotropic silk film; it has rainbow color under orthogonal polarized light; the arrangement of the silk fibroin nanofibers has a helical structure with chiral structural characteristics.
8. A silk fibroin liquid crystal hydrogel, which is obtained by placing the silk fibroin nanofiber liquid crystal suspension according to any one of claims 1 to 3 in hydrochloric acid vapor and sealing it for storage.
9. A silk fibroin liquid crystal aerogel, characterized in that: The hydrogel as claimed in claim 8 is placed in ethanol for solvent exchange, and then freeze-dried to obtain a silk fibroin liquid crystal aerogel.
Citation Information
Patent Citations
Dissolving method for fibroin protein
CN106046133A
Silkworm silk fibroin nanofiber and preparation method thereof
CN106757447A
Method for directly extracting fibroin nanofiber and recovering hydrolyzed silk protein and extracting solution from waste silkworm cocoons
CN114163684A
Preparation method of conductive hydrogel sensor based on polyacrylamide-silk fibroin
CN110845815A
Preparation method and application of silk protein nanofiber
CN113818096A