Antibacterial polyurethane fiber material and preparation method thereof

The antibacterial polyurethane fiber material is prepared through a three-step method, and the antibacterial agent is introduced using the bronopol chain extender, which solves the problem of insufficient binding ability of the antibacterial agent and the matrix, achieves the stability and safety of the antibacterial fiber, and reduces environmental and health threats. , in line with the concept of green chemistry.

CN115961383BActive Publication Date: 2024-10-29TAYHO ADVANCED MATERIALS GRP CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211627012.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-16
Publication Date
2024-10-29
Estimated Expiration
2042-12-16

AI Technical Summary

Technical Problem

The existing PU sterilization materials have weak binding ability of antibacterial agents to the matrix, which leads to the dissolution of chemical substances and harms the environment and human health, and chemical grafting may have adverse effects on the material surface.

Method used

A three-step method is used to prepare antibacterial polyurethane fiber materials. Antibacterial agents are introduced through polymerization and evenly mixed with TPU through composite spinning. Bronopol chain extender is used to introduce polyurethane segments to improve antibacterial stability and maintain material performance to the maximum extent. , to avoid dissolution of antibacterial agents.

Benefits of technology

It improves the binding ability of antibacterial agents to the matrix, reduces threats to the environment and human health, realizes the durable and safe properties of antibacterial fibers, and conforms to the concept of green chemistry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115961383B_ABST
    Figure CN115961383B_ABST
Patent Text Reader

Abstract

The invention discloses an antibacterial polyurethane fiber material and a preparation method thereof, and belongs to the technical field of synthetic materials. The method disclosed by the invention is to mix polycaprolactone and 4,4'-diphenyl diisocyanate and then perform a first prepolymerization reaction, and after the reaction, add an organic solution of bronopol to perform a second prepolymerization reaction to obtain a prepolymer; after the prepolymer is mixed with a chain extender, chain extension and curing cross-linking reaction are performed to obtain a polyurethane material with bulk antibacterial properties; the polyurethane material with bulk antibacterial properties and polyurethane are dissolved in an organic solvent to obtain a spinning solution; the spinning solution is subjected to a spinning process to obtain an antibacterial polyurethane fiber material. The antibacterial polyurethane fiber material obtained by the above preparation method has better antibacterial stability and maintains the various properties of the polyurethane material itself to the maximum extent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of synthetic materials, and in particular relates to an antibacterial polyurethane fiber material and a preparation method thereof. Background Art

[0002] In recent years, bacterial contamination has posed a huge threat to human health and normal production and life. For this reason, a large number of antibiotics have been developed and used, but it is inevitable that a large number of bacteria have developed drug resistance, making it impossible to effectively resist the invasion of microorganisms. Therefore, it is urgent to develop new antibacterial materials to meet the needs of human production and life.

[0003] Polyurethane (PU) is a general term for macromolecular compounds containing repeated carbamate groups on the main chain. It has excellent wear resistance, oil resistance, tear resistance, chemical corrosion resistance, and good biocompatibility. Therefore, it is widely used in various fields, especially in the field of biomedical materials. However, the threat of PU materials to human health and the environment in the process of biomedical application has not been effectively solved, so the application of PU materials has been affected to a certain extent.

[0004] The proliferation of bacteria on the surface of materials will have a serious impact on medical care and industrial production. Therefore, antibacterial materials that can prevent bacterial adhesion and biofilm formation have received widespread attention from researchers. At present, the types of antibacterial agents used in PU bactericidal materials mainly include inorganic antibacterial agents, organic antibacterial agents and natural antibacterial agents. However, considering the processability of materials and the stability of antibacterial properties, organic antibacterial agents have more significant advantages in the preparation of antibacterial materials in related fields. At present, many antibacterial agents are introduced mainly by blending and chemical grafting. However, due to the low molecular weight of most organic antibacterial agents, it is difficult to firmly combine with the matrix material by simple mixing, resulting in the dissolution of chemical substances, which harms the environment and human health. Chemical grafting generally requires the surface of the material to be treated, which may have an adverse effect on the surface of the material. At the same time, the grafting rate of the reaction and the firmness of the functional group's bonding with the interface will also become the main factors limiting its use. Summary of the invention

[0005] In order to overcome the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide an antibacterial polyurethane fiber material and a preparation method thereof, so as to solve the technical problem that the prior art has weak binding ability between the antibacterial agent and the matrix when preparing PU bactericidal materials.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The invention discloses a method for preparing an antibacterial polyurethane fiber material, comprising the following steps:

[0008] S1: mixing polycaprolactone and 4,4'-diphenyl diisocyanate to carry out a first prepolymerization reaction, and after the reaction, adding an organic solution of bronopol to carry out a second prepolymerization reaction to obtain a prepolymer;

[0009] S2: After mixing the prepolymer with the chain extender, chain extension and curing cross-linking reaction are carried out to obtain a polyurethane material with bulk antibacterial properties;

[0010] S3: dissolving the polyurethane material with intrinsic antibacterial properties and polyurethane in an organic solvent to obtain a spinning solution; and subjecting the spinning solution to a spinning process to obtain an antibacterial polyurethane fiber material.

[0011] Furthermore, in S1, the molecular weight of the polycaprolactone is 1000-2000; and the polycaprolactone is vacuum dried at 100-120° C. for 1-2 hours before use.

[0012] Furthermore, in S1, the temperature of the first prepolymerization reaction is 80-90°C, and the time of the first prepolymerization reaction is 1-2h; the temperature of the second prepolymerization reaction is 80-90°C, and the time of the second prepolymerization reaction is 0.5-2h; the molar ratio of OH groups to NCO groups in the prepolymerization reaction is 1:(1.01-1.09).

[0013] Furthermore, in S2, the mass ratio of the prepolymer to the chain extender is (15-30):1; and the chain extender is 1,4-butanediol, 1,6-hexanediol or neopentyl glycol.

[0014] Furthermore, in S2, the temperature of the curing and cross-linking reaction is 70 to 90° C., and the curing and cross-linking reaction time is 12 to 24 hours.

[0015] Furthermore, in S3, the organic solvent is N,N-dimethylformamide or N,N-dimethylacetamide; and the spinning process is electrospinning, wet spinning or dry spinning.

[0016] Furthermore, when the spinning process is electrospinning, the voltage of electrospinning is 15-25 kV, and the solid content of the spinning solution is 15%-25%; when the spinning process is wet spinning or dry spinning, the solid content of the spinning solution is 25%-35%.

[0017] Furthermore, the mass ratio of the polyurethane material with bulk antibacterial properties to the polyurethane in the spinning solution is 1:(0.5-2.0).

[0018] Furthermore, in S3, the polyurethane material with bulk antibacterial properties and the polyurethane are dried at 60 to 80° C. for 12 to 24 hours before use.

[0019] The invention also discloses an antibacterial polyurethane fiber material prepared by the preparation method.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The present invention discloses a method for preparing an antibacterial polyurethane fiber material, firstly, an antibacterial agent is introduced into the polyurethane structure through a polymerization reaction, and then it is uniformly mixed with TPU by composite spinning to obtain a bulk antibacterial fiber or fiber membrane with bronopol chain extension and durable safety characteristics; the present invention adopts a classic three-step method to prepare the polyurethane material, and introduces small molecule bronopol into the polyurethane chain segment in the form of a chain extender through a polymerization reaction. Compared with blending and chemical grafting, the obtained material has better antibacterial stability and maintains the various properties of the polyurethane material itself to the maximum extent. Finally, because the antibacterial fiber material is prepared by polymerization reaction, it mainly kills bacteria by contact during use, and the dissolution and release of the antibacterial agent will not occur, thereby improving the binding ability of the antibacterial agent with the matrix, greatly reducing pollution to the environment and threats to human health, and at the same time following the currently advocated green chemistry concept, it has broad application prospects.

[0022] The present invention also discloses an antibacterial polyurethane fiber material prepared by the above-mentioned preparation method. In terms of the selection of materials in the polyurethane preparation process, using MDI with high reactivity as the hard segment of the polyurethane can effectively reduce the use of catalysts in the synthesis process, making the polymerization reaction more environmentally friendly. In addition, by selecting bronopol with two terminal hydroxyl groups, the hydroxyl group can be directly used as a reactive group to react with isocyanate and introduced into the polyurethane segment without chemical modification, further simplifying the reaction steps in the material preparation process. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a test chart of the antibacterial performance of the antibacterial polyurethane fiber material prepared by the present invention;

[0024] Among them: a, b-control group and experimental group of Staphylococcus aureus; c, d-control group and experimental group of Escherichia coli; e, f-control group and experimental group of Bacillus subtilis;

[0025] Figure 2 This is a test diagram of the dissolution performance of the antibacterial polyurethane fiber material prepared by the present invention;

[0026] Among them: a-Staphylococcus aureus; b-Escherichia coli. DETAILED DESCRIPTION

[0027] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0028] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0029] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible sub-ranges and individual values ​​within the range (including integers and fractions).

[0030] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”

[0031] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0032] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0033] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.

[0034] Example 1

[0035] A method for preparing an antibacterial polyurethane fiber material comprises the following steps:

[0036] S1: Add vacuum-dried polycaprolactone (PCL) into a three-necked flask, then dehydrate and vacuum-dry at 100°C for 2h, add 4,4'-diphenyl diisocyanate (MDI) and mix, and then carry out a first prepolymerization reaction for 1.5h. After the reaction, add an organic solution of bronopol at 85°C for a second prepolymerization reaction for 0.5h to obtain a prepolymer; the molar ratio of OH to NCO groups in the prepolymerization reaction is 1:1.05;

[0037] S2: 141.2 g of the prepolymer and 9.3 g of 1,4-butanediol (BDO) were stirred at high speed for chain extension, poured into a tetrafluoroethylene mold, and cured at 80° C. for 12 h to undergo a curing and cross-linking reaction to obtain a polyurethane material (PBU) with bulk antibacterial properties;

[0038] S3: First, dry PBU and TPU at 80°C for 12 hours; then, dissolve PBU and polyurethane (TPU) in DMF solution at 80°C (PBU:TPU=2:3) to obtain a spinning solution with a solid content of 20%, and then prepare an antibacterial polyurethane fiber material by electrospinning the spinning solution; the voltage of the electrospinning is 15kV.

[0039] Example 2

[0040] A method for preparing an antibacterial polyurethane fiber material comprises the following steps:

[0041] S1: Add polycaprolactone (PCL) with a molecular weight of 2000 into a three-necked flask, then dehydrate and vacuum dry at 120°C for 2 hours, add 4,4'-diphenyl diisocyanate (MDI) and mix, and then carry out a first prepolymerization reaction for 1 hour. After the reaction, add an organic solution of bronopol at 80°C for a second prepolymerization reaction for 0.5 hours to obtain a prepolymer; the molar ratio of OH to NCO groups in the prepolymerization reaction is 1:1.05;

[0042] S2: 147.4 g of the prepolymer and 6.3 g of 1,4-butanediol (BDO) were stirred at high speed for chain extension, poured into a tetrafluoroethylene mold, and cured at 70° C. for 20 h to undergo a curing and cross-linking reaction to obtain a polyurethane material (PBU) with bulk antibacterial properties;

[0043] S3: First, dry PBU and TPU at 75°C for 20 hours; then, dissolve PBU and polyurethane (TPU) in DMF solution at 80°C (PBU:TPU=2:3) to obtain a spinning solution with a solid content of 20%, and then prepare an antibacterial polyurethane fiber material by electrospinning the spinning solution; the voltage of the electrospinning is 15kV.

[0044] Example 3

[0045] A method for preparing an antibacterial polyurethane fiber material comprises the following steps:

[0046] S1: Add polycaprolactone (PCL) with a molecular weight of 1000 into a three-necked flask, then dehydrate and vacuum dry at 100°C for 2 hours, add 4,4'-diphenyl diisocyanate (MDI) and mix, and then carry out a first prepolymerization reaction for 1.5 hours. After the reaction, add an organic solution of bronopol at 90°C for a second prepolymerization reaction for 0.5 hours to obtain a prepolymer; the molar ratio of OH to NCO groups in the prepolymerization reaction is 1:1.05;

[0047] S2: 144.8 g of the prepolymer and 7.4 g of 1,4-butanediol (BDO) were stirred at high speed for chain extension, poured into a tetrafluoroethylene mold, and cured at 80° C. for 12 h to undergo a curing and cross-linking reaction to obtain a polyurethane material (PBU) with bulk antibacterial properties;

[0048] S3: First, dry PBU and TPU at 60°C for 24h; then, dissolve PBU and polyurethane (TPU) in DMF solution at 80°C (PBU:TPU=2:3) to obtain a spinning solution with a solid content of 20%, and then prepare an antibacterial polyurethane fiber material by electrospinning the spinning solution; the voltage of the electrospinning is 25kV.

[0049] Example 4

[0050] A method for preparing an antibacterial polyurethane fiber material comprises the following steps:

[0051] S1: Add polycaprolactone (PCL) with a molecular weight of 1000 into a three-necked flask, then dehydrate at 100°C for 2h and vacuum dry, then add 4,4'-diphenyl diisocyanate (MDI) and mix, and then carry out a first prepolymerization reaction for 1.5h. After the reaction, add an organic solution of bronopol at 85°C for a second prepolymerization reaction for 0.5h to obtain a prepolymer; the molar ratio of OH to NCO groups in the prepolymerization reaction is 1:1.03;

[0052] S2: 144.8 g of the prepolymer and 7.4 g of 1,4-butanediol (BDO) were stirred at high speed for chain extension, poured into a tetrafluoroethylene mold, and cured at 80° C. for 12 h to undergo a curing and cross-linking reaction to obtain a polyurethane material (PBU) with bulk antibacterial properties;

[0053] S3: First, dry PBU and TPU at 65°C for 20 hours; then, dissolve PBU and polyurethane (TPU) in DMF solution at 80°C (PBU:TPU=2:3) to obtain a spinning solution with a solid content of 20%, and then prepare an antibacterial polyurethane fiber material by electrospinning the spinning solution; the voltage of the electrospinning is 15kV.

[0054] Example 5

[0055] A method for preparing an antibacterial polyurethane fiber material comprises the following steps:

[0056] S1: Add polycaprolactone (PCL) with a molecular weight of 1000 into a three-necked flask, then dehydrate and vacuum dry at 100°C for 2 hours, add 4,4'-diphenyl diisocyanate (MDI) and mix, and then carry out a first prepolymerization reaction for 1.5 hours. After the reaction, add an organic solution of bronopol at 85°C for a second prepolymerization reaction for 0.5 hours to obtain a prepolymer; the molar ratio of OH to NCO groups in the prepolymerization reaction is 1:1.01;

[0057] S2: 144.8 g of the prepolymer and 7.4 g of 1,4-butanediol (BDO) were stirred at high speed for chain extension, poured into a tetrafluoroethylene mold, and cured at 80° C. for 12 h to undergo a curing and cross-linking reaction to obtain a polyurethane material (PBU) with bulk antibacterial properties;

[0058] S3: First, dry PBU and TPU at 80°C for 12 hours; then, dissolve PBU and polyurethane (TPU) in DMF solution at 80°C (PBU:TPU=2:3) to obtain a spinning solution with a solid content of 20%, and then prepare an antibacterial polyurethane fiber material by electrospinning the spinning solution; the voltage of the electrospinning is 15kV.

[0059] Example 6

[0060] The difference from Example 1 is that the solid content of the spinning solution in this example is 15%, and the other parameters and steps are the same as those in Example 1, thereby obtaining an antibacterial polyurethane fiber material.

[0061] Example 7

[0062] In this embodiment, the preparation method of PBU is as shown in Example 1. Then, PBU and TPU are dissolved in DMF solution at 80°C (PBU: TPU = 2: 3) to prepare a spinning solution with a mass fraction of 25%, and an antibacterial polyurethane film is prepared by an electrospinning method. The concentration of the electrospinning solution at this mass fraction is too high, resulting in a high viscosity, so that it is difficult to form a Taylor cone structure during the spinning process, and spinning is difficult.

[0063] Example 8

[0064] A method for preparing an antibacterial polyurethane fiber material comprises the following steps:

[0065] S1: Add polycaprolactone (PCL) with a molecular weight of 1000 into a three-necked flask, then dehydrate and vacuum dry at 120°C for 2 hours, add 4,4'-diphenyl diisocyanate (MDI) and mix, and then carry out a first prepolymerization reaction for 2 hours. After the reaction, add an organic solution of bronopol at 80°C for a second prepolymerization reaction for 2 hours to obtain a prepolymer; the molar ratio of OH to NCO groups in the prepolymerization reaction is 1:1.09;

[0066] S2: After chain extension by high-speed stirring of 148.3 g of prepolymer and 5.1 g of neopentyl glycol, the mixture was poured into a tetrafluoroethylene mold and cured at 90° C. for 24 h to undergo a curing and cross-linking reaction, thereby obtaining a polyurethane material (PBU) with bulk antibacterial properties;

[0067] S3: First, dry PBU and TPU at 80°C for 12 hours; then, dissolve PBU and polyurethane (TPU) in DMF solution at 80°C (PBU:TPU=1:0.5) to obtain a spinning solution with a solid content of 25%, and then prepare an antibacterial polyurethane fiber material by a wet spinning method.

[0068] Example 9

[0069] A method for preparing an antibacterial polyurethane fiber material comprises the following steps:

[0070] S1: Add polycaprolactone (PCL) with a molecular weight of 1000 into a three-necked flask, then dehydrate and vacuum dry at 120°C for 2 hours, add 4,4'-diphenyl diisocyanate (MDI) and mix, and then carry out a first prepolymerization reaction for 2 hours. After the reaction, add an organic solution of bronopol at 90°C for a second prepolymerization reaction for 0.5 hours to obtain a prepolymer; the molar ratio of OH to NCO groups in the prepolymerization reaction is 1:1.09;

[0071] S2: 146.3 g of the prepolymer and 10.1 g of 1,6-hexanediol were stirred at high speed for chain extension, poured into a tetrafluoroethylene mold, and cured at 90° C. for 24 h to undergo a curing and cross-linking reaction to obtain a polyurethane material (PBU) with bulk antibacterial properties;

[0072] S3: First, PBU and TPU are dried at 60°C for 12 hours; then, PBU and polyurethane (TPU) are dissolved in DMF solution at 60°C (PBU:TPU=1:2) to obtain a spinning solution with a solid content of 35%, and then the spinning solution is prepared by a dry spinning method to obtain an antibacterial polyurethane fiber material.

[0073] Comparative Example 1

[0074] In this embodiment, the preparation method of PBU is as shown in Example 1. Then, PBU and TPU are dissolved in DMF solution at 80°C (PBU: TPU = 4: 1) to prepare a spinning solution with a mass fraction of 20%, and an antibacterial polyurethane film is prepared by an electrospinning method. The spinnability of the spinning solution at this ratio is poor, and the mechanical properties of the electrospinning membrane formed are poor.

[0075] Figure 1 The figure shows the antibacterial performance test of the antibacterial polyurethane fiber material prepared by the present invention. It can be seen from the figure that the experimental group co-cultured the experimental bacteria with the antibacterial polyurethane fiber material by using the contact antibacterial method, while the bacteria in the control group were not added with any material. After 12 hours of contact culture, the bacterial solution was taken out and coated on the agar medium to observe the colony density. Figure 1 a~ Figure 1 It can be seen that the antibacterial polyurethane fiber material synthesized by the present invention has a strong killing ability against Staphylococcus aureus, Escherichia coli and Bacillus subtilis, and the sterilization rate can reach more than 99.99%.

[0076] Figure 2 The figure shows the dissolution performance test of the antibacterial polyurethane fiber material prepared by the present invention. First, the antibacterial polyurethane fiber material is soaked and washed 10 times, and then the material is cut and placed in the middle of the agar medium evenly coated with bacterial solution to observe the dissolution performance of the material. Figure 2 a~ Figure 2 b It can be seen that no antibacterial zone appears around the antibacterial polyurethane fiber material, that is, no antibacterial substance is dissolved, which shows that the antibacterial agent involved in the present invention is firmly combined with the base material, is not likely to cause potential harm to human health or the environment, and has good safety.

[0077] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A method for preparing an antibacterial polyurethane fiber material, characterized in that: The following steps are involved: S1: mixing polycaprolactone and 4,4'-diphenyl diisocyanate to carry out a first prepolymerization reaction, and after the reaction, adding an organic solution of bronopol to carry out a second prepolymerization reaction to obtain a prepolymer; S2: After mixing the prepolymer with the chain extender, chain extension and curing cross-linking reaction are carried out to obtain a polyurethane material with bulk antibacterial properties; S3: dissolving the polyurethane material with bulk antibacterial properties and the polyurethane in an organic solvent to obtain a spinning solution; and subjecting the spinning solution to a spinning process to obtain an antibacterial polyurethane fiber material; In S1, the temperature of the first prepolymerization reaction is 80-90°C, and the time of the first prepolymerization reaction is 1-2 h; the temperature of the second prepolymerization reaction is 80-90°C, and the time of the second prepolymerization reaction is 0.5-2 h; the molar ratio of OH group to NCO group in the prepolymerization reaction is 1:(1.01-1.09); In S2, the temperature of the chain extension and curing cross-linking reaction is 70-90° C., and the chain extension and curing cross-linking reaction time is 12-24 hours; In S2, the mass ratio of the prepolymer to the chain extender is (15-30):1; the chain extender is 1,4-butanediol, 1,6-hexanediol or neopentyl glycol.

2. The method for preparing an antibacterial polyurethane fiber material according to claim 1, characterized in that: In S1, the molecular weight of the polycaprolactone is 1000-2000; the polycaprolactone is vacuum dried at 100-120° C. for 1-2 h before use.

3. The method for preparing an antibacterial polyurethane fiber material according to claim 1, characterized in that: In S3, the organic solvent is N,N-dimethylformamide or N,N-dimethylacetamide; and the spinning process is electrospinning, wet spinning or dry spinning.

4. The method for preparing an antibacterial polyurethane fiber material according to claim 3, characterized in that: When the spinning process is electrospinning, the voltage of electrospinning is 15-25 kV, and the solid content of the spinning solution is 15%-25%; when the spinning process is wet spinning or dry spinning, the solid content of the spinning solution is 25%-35%.

5. The method for preparing an antibacterial polyurethane fiber material according to claim 4, characterized in that: The mass ratio of the polyurethane material with bulk antibacterial properties to the polyurethane in the spinning solution is 1:(0.5-2.0).

6. The method for preparing an antibacterial polyurethane fiber material according to claim 1, characterized in that: In S3, the polyurethane material with bulk antibacterial properties and the polyurethane are dried at 60-80° C. for 12-24 h before use.

7. An antibacterial polyurethane fiber material, characterized in that: The antibacterial polyurethane fiber material is prepared by the method for preparing an antibacterial polyurethane fiber material according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Surgical suture with antibacterial and shape memory functions and preparation method thereof

    CN112358595A

  • Preparation method and application of durable antibacterial and mildew-proof regenerated leather

    CN114164680A