A Na2FeP2O7@C nanotube array / carbon cloth composite and preparation method thereof and sodium ion battery
Through the preparation of Na2FeP2O7@C nanotube array/carbon cloth composite, the flexibility and performance problems of sodium-ion battery cathode materials are solved, flexible bending, folding and high-rate performance are achieved, and cycle stability and conductivity are improved.
Patent Information
- Application Number
- CN202310060066.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-18
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-01-18
AI Technical Summary
Existing sodium-ion battery cathode materials are difficult to achieve flexible bending and folding, and have poor cycle stability and rate performance, mainly due to complex preparation and low electronic conductivity.
Using the preparation method of Na2FeP2O7@C nanotube array/carbon cloth composite, a regular nanotube array structure is formed through hydrothermal reaction and sintering process, reducing the dependence on conductive agents and binders, and improving the conductivity and structural stability of the material. sex.
It achieves the flexible bending and folding capabilities of sodium-ion batteries, significantly improves the cycle life and rate performance of the material, reduces internal interface resistance, and enhances electronic conductivity and sodium ion diffusion channels.
Smart Images

Figure CN115966679B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of positive electrode materials for sodium ion batteries, and in particular to a Na2FeP2O7@C nanotube array / carbon cloth composite and a preparation method thereof, and a sodium ion battery. Background Art
[0002] Sodium-ion batteries have abundant resources and low costs, and have great development advantages in large-scale energy storage and conversion fields such as smart grids and low-speed electric vehicles. In recent years, people have higher and higher requirements for the miniaturization, diversity and variability of electronic products. With the advent of flexible electronic products such as rollable displays, electronic shirts and roll-screen mobile phones, researchers have paid extensive attention to flexible electronic technology. The solvation radius of sodium ions is smaller than that of lithium ions, and they have better interfacial diffusion ability. At the same time, the ionic conductivity of sodium salt electrolytes is higher than that of lithium salt electrolytes at the same concentration. This means that sodium-ion batteries have better rate performance. Current sodium-ion batteries are difficult to bend and fold, and it is difficult to meet the development needs of flexible electronic devices. Therefore, it is of great significance to develop flexible sodium-ion batteries and electrode materials.
[0003] Iron-based phosphate cathode materials have attracted widespread attention due to their high energy density, abundant raw material resources, low price and good safety. Phosphate-based sodium-ion battery cathode materials are a type of polyanion-type materials with a three-dimensional framework structure composed of strong covalent bonds. Since the polyanions in iron-based phosphate cathode materials have an adjustable inductive effect on redox couples, it is easy to increase the potential of such materials and obtain high-potential cathode materials. In addition, the structure of iron-based phosphate cathode materials is relatively stable, which is conducive to long cycles and has high safety. These advantages make them have a broad development prospect in large-scale fixed energy storage systems. Na2FeP2O7 cathode materials have the advantages of high energy density, abundant raw material resources, low price and high cost performance.
[0004] However, flexible iron-based sodium phosphate battery cathode materials are limited by the complexity of preparation and the difficulty in accurately obtaining nano-array structured sodium phosphate battery cathode materials, resulting in less research. Currently, binder-free iron-based sodium phosphate battery cathodes mostly use coating and impregnation methods, which have poor bonding with the substrate, making it difficult to achieve flexible bending and folding, and have poor cycle stability. Low-cost Na2FeP2O7 cathode materials also face problems such as difficulty in precise synthesis, low electronic conductivity, multiple interfaces between active particles inside the electrode, and large interface resistance, which seriously affect the long cycle and rate performance of the material. Summary of the invention
[0005] In order to overcome the deficiencies of the above prior art, the purpose of the present invention is to provide a method for preparing a Na2FeP2O7@C nanotube array / carbon cloth composite to avoid the problems of long cycle and poor rate performance of Na2FeP2O7 positive electrode materials.
[0006] Another object of the present invention is to provide a Na2FeP2O7@C nanotube array / carbon cloth composite.
[0007] Another object of the present invention is to provide a sodium ion battery.
[0008] The purpose of the present invention is achieved through the following technical solutions:
[0009] A method for preparing a Na2FeP2O7@C nanotube array / carbon cloth composite comprises the following steps:
[0010] Cobalt chloride, nickel chloride and urea are dissolved in water, stirred evenly in a reactor and then carbon cloth is added. When the hydrothermal reaction is complete, the product is washed and dried to obtain a precursor array. The precursor array is placed in a ferric chloride solution, and the mixture is sequentially kept warm, washed and dried to obtain a FeOOH nanotube array / carbon cloth composite. The FeOOH nanotube array / carbon cloth composite is immersed in a mixed solution of glucose and sodium pyrophosphate, naturally air-dried, and then sintered at high temperature under a protective atmosphere to obtain a Na2FeP2O7@C nanotube array / carbon cloth composite.
[0011] Preferably, in the mixed solution, the concentration of the glucose solution is 0.6-1.0 mol / L, the concentration of the sodium pyrophosphate solution is 1.0-2.0 mol / L, and the soaking time is 12-18 hours.
[0012] Preferably, the high temperature sintering temperature is 400-600° C., and the high temperature sintering time is 3-5 hours.
[0013] Preferably, the protective atmosphere is argon.
[0014] Preferably, the concentration of the cobalt chloride is 0.45-0.65 mol / L, the concentration of the nickel chloride is 0.25-0.35 mol / L, and the concentration of the urea is 1.8-2.2 mol / L.
[0015] Preferably, the filling degree of the reactor is 70-90%, the washing is performed with deionized water and ethanol solution, the drying temperature is 50-100°C, the drying time is 10-14 hours, the hydrothermal reaction time is 5-12 hours, the hydrothermal reaction temperature is 100-140°C, and the size of the carbon cloth is 3cm×6cm.
[0016] Preferably, the concentration of the ferric chloride solution is 0.03-0.06 mol / L.
[0017] Preferably, the insulation temperature is 40-70° C., and the insulation time is 8-14 hours.
[0018] A Na2FeP2O7@C nanotube array / carbon cloth composite is prepared by the above-mentioned preparation method of a Na2FeP2O7@C nanotube array / carbon cloth composite.
[0019] Preferably, the diameter of the nanotube is 100-200 nanometers and the length is 3-6 micrometers.
[0020] A sodium ion battery, wherein the positive electrode of the sodium ion battery comprises the Na2FeP2O7@C nanotube array / carbon cloth composite flexible electrode.
[0021] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0022] (1) The present invention provides a method for preparing a Na2FeP2O7@C nanotube array / carbon cloth composite with regular morphology by in-situ deposition and etching of a binary basic carbonate precursor of nickel and cobalt, combined with capillary adsorption and heat treatment, and the preparation method is controllable.
[0023] (2) The Na2FeP2O7@C nanotube array / carbon cloth composite prepared by the present invention does not require coating, reduces the process, improves the contact between the active material and the current collector, has the advantage of three-dimensional structure to transmit electrons, and greatly improves the rate performance and cycle life of the iron-based phosphate positive electrode material; the unique micro-nano structure enables the Na2FeP2O7@C negative electrode to have sufficient void space to buffer the volume change, which is conducive to the infiltration of the electrolyte and promotes the coordinated transmission of sodium ions and electrons, thereby improving the rate performance of the material. Secondly, the carbon coating layer formed by the decomposition of the adsorbed glucose during the heat treatment process improves the overall conductivity of the Na2FeP2O7 material and maintains the structural integrity of the Na2FeP2O7 nanotube array during the charge and discharge process.
[0024] (3) The Na2FeP2O7@C nanotube array / carbon cloth composite prepared by the present invention does not require a conductive agent and a binder, can truly reflect the sodium ion storage properties of the material itself, and is conducive to studying the sodium ion storage mechanism of the material. The Na2FeP2O7@C nanotube array has excellent bonding ability with the substrate and can achieve flexible bending and folding.
[0025] (4) In the Na2FeP2O7@C nanotube array / carbon cloth composite prepared by the present invention, the nanotube array structure greatly increases the contact area between the electrode material and the electrolyte, providing more diffusion channels for sodium ion batteries. At the same time, the carbon-coated structure can effectively improve the low electronic conductivity of the material, the large number of interfaces between the active particles inside the electrode, and the large interface resistance. The one-dimensional nanotube structure improves the problem of many interfaces and large interface resistance between the active particles inside Na2FeP2O7, which is conducive to the self-buffering volume expansion during the sodium insertion and extraction process, and then forms a stable SEI film; the nanotube array structure is conducive to the infiltration of the electrolyte, shortens the diffusion distance of sodium ions, and is conducive to reducing the sodium ion diffusion energy barrier and realizing efficient sodium ion transmission; the one-dimensional conductive carbon shell not only stabilizes the overall structure of the material, but also greatly improves the electronic conductivity of the composite electrode material and reduces the internal resistance of the system. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is the SEM image of the nickel and cobalt binary basic carbonate precursor array.
[0027] Figure 2 This is the SEM image of the FeOOH nanoarray / carbon cloth composite.
[0028] Figure 3 This is the XRD pattern of Na2FeP2O7@C nanotube array / carbon cloth composite.
[0029] Figure 4 This is the SEM image of the Na2FeP2O7@C nanotube array / carbon cloth composite.
[0030] Figure 5 TEM image of Na2FeP2O7@C nanotube array / carbon cloth composite.
[0031] Figure 6 This is the energy spectrum scan of Na2FeP2O7@C nanotube TEM.
[0032] Figure 7 This is the CV diagram of Na2FeP2O7@C nanotube array / carbon cloth composite.
[0033] Figure 8 This is the voltage-capacity curve of the Na2FeP2O7@C nanotube array / carbon cloth composite.
[0034] Fig. 9 This is the cycling performance diagram of Na2FeP2O7@C nanotube array / carbon cloth composite.
[0035] Fig.10 This is the rate performance diagram of Na2FeP2O7@C nanotube array / carbon cloth composite. DETAILED DESCRIPTION
[0036] The purpose of the present invention is further described in detail below with reference to the accompanying drawings and specific examples. The examples cannot be described one by one here, but the implementation methods of the present invention are not therefore limited to the following examples.
[0037] Embodiment 1
[0038] The present invention will be further described below in conjunction with specific embodiments.
[0039] Take 80 mL of a mixed solution, which is composed of a mixed solution of 0.2 mol / L nickel chloride, 0.4 mol / L cobalt chloride and 2.0 mol / L urea, add carbon cloth, stir evenly, put into a reactor with a volume of 100 mL, and perform hydrothermal reaction at 120° C. for 6 hours, cool to room temperature, wash the product with deionized water and ethanol, dry at 80° C., and obtain a precursor array after drying. Figure 1 As shown; the obtained precursor array is placed in a 0.05 mol / L ferric chloride solution at 50°C for 12 hours for in-situ deposition and etching, washed with deionized water and ethanol, and dried at 60°C for 12 hours to obtain a flexible FeOOH nanotube array / carbon cloth composite, as shown Figure 2 As shown; the FeOOH nanotube array / carbon cloth composite obtained above was immersed in 0.5 mol / L glucose and sodium pyrophosphate solution for 12 hours by in-situ deposition and etching and glucose solution adsorption and carbon coating, naturally air-dried, and finally sintered at 500°C for 3 hours to obtain a flexible Na2FeP2O7@C nanotube array / carbon cloth composite, as shown Figure 3 shown.
[0040] The Na2FeP2O7@C nanotube array / carbon cloth was cut into discs as the positive electrode, and the sodium sheet was used as the negative electrode. The button cell was assembled in an argon atmosphere glove box for testing. The test conditions were: the charge and discharge cut-off voltage was 2.0 V to 4.0 V, and the scan rate was 0.1 mV s -1 The cyclic voltammetry curve obtained by the test is shown in Figure 7 .
[0041] SEM image of Na2FeP2O7@C nanotube array / carbon cloth composite Figure 4 As shown, from Figure 4 From the scanning electron microscope image, it can be seen that the Na2FeP2O7@C nanotubes have a regular morphology and are evenly attached to the carbon fibers of the carbon cloth, proving that the prepared Na2FeP2O7@C is a hollow nanotube.
[0042] TEM image of Na2FeP2O7@C nanotube array / carbon cloth composite Figure 5As shown by Figure 5 It can be seen that the nanotubes are wrapped by a carbon shell and the diameter of the nanotubes is about 200 nm.
[0043] The TEM spectrum scan of a single Na2FeP2O7@C nanotube is shown in the figure below. Figure 6 As shown by Figure 6 It can be seen that Na, Fe, P, and O elements are evenly distributed on the tube wall, and the C element is more distributed in the nanotubes because more glucose solution is adsorbed into the nanotubes and carbonized during the subsequent sintering process.
[0044] CV graph of Na2FeP2O7@C nanotube array / carbon cloth composite Figure 7 As shown by Figure 7 It can be seen that the Na2FeP2O7@C cathode has two obvious sodium insertion reduction peaks at 2.88 V and 2.36 V, and two obvious sodium removal oxidation peaks at 2.56 V and 3.0 V. The CV curves from the second to the fifth cycle have good overlap, indicating that the Na2FeP2O7@C array cathode has good cycle performance.
[0045] The voltage-capacity curve of Na2FeP2O7@C nanotube array / carbon cloth composite is shown in Figure 8 As shown by Figure 8 It can be seen that the composite material prepared in this example has an initial discharge capacity of 95 mAh / g and has good cycle reversibility.
[0046] The cycling performance of Na2FeP2O7@C nanotube array / carbon cloth composite is shown in the figure Fig. 9 As shown by Fig. 9 It can be seen that the charge and discharge current density is 1000mA / g, and the composite material prepared in this embodiment shows a capacity of 80mAh / g and good cycle stability after 2400 cycles. The unique micro-nano structure enables the Na2FeP2O7@C negative electrode to have sufficient void space to buffer the volume change, which is beneficial to the infiltration of the electrolyte and promotes the coordinated transmission of sodium ions / electrons, thereby improving the rate performance of the material. Secondly, the carbon coating layer formed by the decomposition of adsorbed glucose during the heat treatment process improves the overall conductivity of the Na2FeP2O7 material and maintains the structural integrity of the Na2FeP2O7@C nanotube array during the charge and discharge process.
[0047] The rate performance of Na2FeP2O7@C nanotube array / carbon cloth composite is shown in the figure Fig.10 As shown by Fig.10It can be seen that the charge and discharge current density is 50, 100, 200, 500, 1000, 2000mA / g (1C = 100mA / g). The prepared Na2FeP2O7@C composite material exhibits a specific capacity of 96.4, 93.2, 90.3, 82.2, 73.9, and 62.8mAh / g under 0.5C, 1C, 2C, 5C, 10C, and 20C, respectively. When the charge and discharge current density returns to the 0.5C state, the Na2FeP2O7@C composite material can still maintain a specific capacity of 95mAh / g. The nanotube array structure design can eliminate the influence of the binder and avoid the problems of multiple interfaces and high resistance between Na2FeP2O7 particles in the traditional electrode. Compared with the traditional film and particle structure electrode materials, the electrode with a three-dimensional ordered film structure composed of this array has one-dimensional electron guidance and sodium ion diffusion stress release space, which can effectively prevent the material from pulverizing and failing. Through the carbon coating surface modification process, the rate performance is further improved, giving Na2FeP2O7@C the performance of fast charging and discharging and long life.
[0048] The above specific implementation modes are preferred embodiments of the present invention and cannot be used to limit the present invention. Any other changes or other equivalent replacement methods that do not deviate from the technical solution of the present invention are included in the protection scope of the present invention.
Claims
1. A sodium ion battery, characterized in that: The Na2FeP2O7@C nanotube array / carbon cloth composite is used as the positive electrode and the sodium sheet is used as the negative electrode; the preparation method of the Na2FeP2O7@C nanotube array / carbon cloth composite comprises the following steps: Dissolve cobalt chloride, nickel chloride and urea in water, stir evenly in a reactor and then add carbon cloth, when the hydrothermal reaction is complete, wash and dry the product to obtain a precursor array; put the precursor array into a ferric chloride solution, keep warm, wash and dry it in sequence to obtain a FeOOH nanotube array / carbon cloth composite; soak the FeOOH nanotube array / carbon cloth composite in a mixed solution containing 0.5 mol / L glucose and sodium pyrophosphate, dry it naturally, and then sinter it under a protective atmosphere to obtain a Na2FeP2O7@C nanotube array / carbon cloth composite; The soaking time is 12 to 18 hours; The sintering temperature is 500° C., and the sintering time is 3 hours.
2. A sodium ion battery according to claim 1, characterized in that: The concentration of the cobalt chloride is 0.45-0.65 mol / L, the concentration of the nickel chloride is 0.25-0.35 mol / L, and the concentration of the urea is 1.8-2.2 mol / L.
3. A sodium ion battery according to claim 1, characterized in that: The filling degree of the reactor is 70-90%, the size of the carbon cloth is 3 cm×6 cm, the time of the hydrothermal reaction is 5-12 hours, the temperature of the hydrothermal reaction is 100-140°C, and the drying temperature is 50-100°C.
4. A sodium ion battery according to claim 1, characterized in that: The concentration of the ferric chloride solution is 0.03-0.06 mol / L.
5. A sodium ion battery according to claim 1, characterized in that: The insulation temperature is 40-70° C., and the insulation time is 8-14 hours.
6. A sodium ion battery according to claim 1, characterized in that: The protective atmosphere is argon.